A waterproof coating containing modified silicone rubber and a preparation method thereof

By using modified silicone rubber and phenolic resin in waterproof coatings, combined with specific preparation methods, the problem of performance reduction of existing coatings due to bacterial corrosion is solved, better waterproof and antibacterial effects are achieved, and service life is extended .

CN118599427BActive Publication Date: 2024-11-12JUNXIU NEW MATERIAL TECH (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410854100.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-12
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing waterproof coatings are prone to deterioration of waterproof and fire resistance due to bacterial corrosion after long-term use, and have insufficient antibacterial effects, which affects service life.

Method used

Using a combination of modified silicone rubber, modified phenolic resin, talc powder, dipropylene glycol butyl ether film forming additive, polysiloxane defoaming agent and ammonium acrylate wetting agent, a combination of high-efficiency waterproof and antibacterial coatings are formed through specific preparation methods. .

Benefits of technology

It significantly improves the waterproof performance and antibacterial effect of the coating, extends its service life, and effectively prevents the penetration of moisture and harmful ions through the hydrophobic membrane structure of silicon oxygen chains and phenolic resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917597270000081
    Figure BDA0004917597270000081
  • Figure BDA0004917597270000091
    Figure BDA0004917597270000091
Patent Text Reader

Abstract

The invention relates to the technical field of waterproof coatings, and discloses a waterproof coating containing modified silicone rubber and a preparation method thereof. The invention obtains a waterproof coating containing modified silicone rubber by mixing and stirring modified silicone rubber, modified phenolic resin, talcum powder, dipropylene glycol butyl ether film-forming aid, polysiloxane defoamer, acrylate ammonium salt wetting agent, and water, stirring evenly, and standing at room temperature. The silicone rubber in the modified silicone rubber itself has a good waterproof effect; the siloxane therein and the siloxane of the modified phenolic resin play a waterproof role; the basic structure of the phenolic resin is composed of benzene rings and hydroxyl groups, and these hydrophobic groups make the phenolic resin have a natural ability to repel moisture, which plays a good waterproof effect; the quaternary ammonium salt contained therein has a good antibacterial effect, which plays a good antibacterial role in the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coatings, in particular to a waterproof coating containing modified silicone rubber and a preparation method thereof. Background Art

[0002] During the long-term use of building materials, moisture in the air will directly affect their function and service life. Waterproof engineering can be divided into structural waterproofing and material waterproofing according to the mode of action. Waterproof coating is a kind of coating, which belongs to material waterproofing. For example, patent CN117965070B discloses a flame retardant waterproof coating for wood and its preparation method, which has excellent flame retardant and waterproof properties. Most importantly, after being coated on the surface of the substrate, the coating will not fall off after a certain amount of wear and tear, which will greatly reduce the waterproof and fireproof properties of the coating, and can greatly extend the service life of the coating; however, the antibacterial effect is not improved, and the coating will be corroded by bacteria if it is exposed to the air for a long time, which will reduce the service life of the coating. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies of the prior art, the present invention provides a waterproof coating containing modified silicone rubber and a preparation method thereof, which has good waterproof and antibacterial effects.

[0005] (II) Technical solution

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a waterproof coating containing modified silicone rubber, comprising the following components by weight: 8-12 parts by weight of modified silicone rubber, 6-10 parts by weight of modified phenolic resin, 2-3 parts by weight of talcum powder, 1-2 parts by weight of dipropylene glycol butyl ether film-forming aid, 0.2-0.5 parts by weight of polysiloxane defoamer, 0.4-0.7 parts by weight of ammonium acrylate wetting agent, and 12-16 parts by weight of water.

[0007] Preferably, the preparation method of the modified silicone rubber is:

[0008] (1) adding a polymerization inhibitor, butylated hydroxytoluene, a tetrahydrofuran solution of chloroplatinic acid, and acrylic acid to an N,N-dimethylformamide solvent, stirring evenly, then adding silicone rubber, ultrasonically dispersing evenly, reacting at 65-80° C. for 6-10 hours, cooling after completion, centrifuging, washing, and drying to obtain a carboxylated silicone rubber;

[0009] (2) adding diethanolamine and double-ended epoxy silicone oil into a reactor filled with isopropanol solvent, reacting at 55-70° C. for 14-18 hours, concentrating after completion, and washing with methanol to obtain intermediate 1;

[0010] (3) Adding intermediate 1 and carboxylated silicone rubber to N,N-dimethylformamide solvent, stirring evenly, and then adding p-toluenesulfonic acid catalyst, reacting at 80-95° C. for 5-8 hours, and then distilling under reduced pressure, filtering and drying to obtain intermediate 2;

[0011] (4) Add 10-12 parts by weight of octadecane chloride and 8-15 parts by weight of intermediate 2 into N,N-dimethylformamide solvent, react at 85-100° C. for 4-7 hours, concentrate after the reaction, and wash with methanol to obtain modified silicone rubber.

[0012] Preferably, the mass ratio of the polymerization inhibitor dibutyl hydroxytoluene, the catalyst chloroplatinic acid, acrylic acid, and the silicone rubber in (1) is 0.01-0.03:0.02-0.03:1:1.1-1.3.

[0013] Preferably, the mass ratio of diethanolamine to double-terminal epoxy silicone oil in (2) is 1.5-2.2:1.

[0014] Preferably, the mass ratio of the intermediate 1, carboxylated silicone rubber and p-toluenesulfonic acid catalyst in (3) is 1:1.2-1.4:0.02-0.04.

[0015] Preferably, the preparation method of the modified phenolic resin is:

[0016] S1. 5-8 parts by weight of intermediate 1, 1-1.5 parts by weight of pyridine, and 7-10 parts by weight of p-methoxybenzoyl chloride are added to a dichloromethane solvent at -5°C to -2°C, and then reacted at 25-40°C for 8-14h, the solvent is concentrated, and the filter cake is washed to obtain intermediate 3;

[0017] S2. 10-13 parts by weight of intermediate 3 is added to a dichloromethane solvent, 0.8-1.4 parts by weight of boron tribromide is added dropwise at -23°C to -10°C, the reaction is continued for 15-20 hours, and then 5-7 parts by weight of methanol are added dropwise to terminate the reaction, the solution is poured into ice water to precipitate, filtered, the filter cake is washed, and recrystallized to obtain phenolic silane;

[0018] S3. Add 7-12 parts by weight of phenolic silane, 10-16 parts by weight of phenol, and 18-30 parts by weight of formaldehyde aqueous solution into the reactor, stir evenly, then add 0.9-1.2 parts by weight of oxalic acid as a catalyst, react at 60-85°C for 5-9h, let stand to separate, filter, wash with water and dry to obtain a modified phenolic resin.

[0019] Preferably, the mass fraction of the aqueous solution of formaldehyde in S3 is 38-41%.

[0020] Preferably, the preparation method of the waterproof coating containing modified silicone rubber comprises the following steps: mixing and stirring the modified silicone rubber, modified phenolic resin, talcum powder, dipropylene glycol butyl ether film-forming aid, polysiloxane defoaming agent, ammonium acrylate wetting agent, and water; after stirring evenly, standing at room temperature for 3-4 hours to obtain the waterproof coating containing modified silicone rubber.

[0021] (III) Beneficial technical effects

[0022] The invention obtains a waterproof coating containing modified silicone rubber by mixing and stirring modified silicone rubber, modified phenolic resin, talcum powder, dipropylene glycol butyl ether film-forming aid, polysiloxane defoamer, ammonium acrylate wetting agent and water, stirring evenly, and standing at room temperature.

[0023] The silicone rubber in the modified silicone rubber itself has a good waterproof effect, because the silicon-oxygen chain segments and organic groups in the silicone rubber form a hydrophobic layer on the surface of the substrate, making it difficult for water molecules to penetrate. The silicone rubber reacts with water vapor in the air to generate a hydrophobic silicone resin film, thereby preventing moisture and harmful ions from penetrating into the interior of the substrate; the siloxane and the siloxane of the modified phenolic resin react with water vapor in the air to also generate a silicone resin film, which plays a waterproof role; the double-ended epoxy silicon reacts with diethanolamine to generate a large number of hydroxyl groups, which further react with carboxylated silicone rubber to increase the degree of substitution of silicone rubber and make the waterproof effect better; the basic structure of the phenolic resin is composed of benzene rings and hydroxyl groups. These hydrophobic groups give the phenolic resin a natural ability to repel moisture and play a good waterproof effect; the quaternary ammonium salt contained therein has a good antibacterial effect and plays a good antibacterial role in the coating. DETAILED DESCRIPTION

[0024] Add 12.7g of octamethylcyclotetrasiloxane and 1.1g of 1,3-diglycidyloxypropyl-1,1,3,3-tetramethyldisiloxane to the reaction kettle, add 10mg of catalyst tetramethylammonium hydroxide in a nitrogen atmosphere, raise the temperature to 120°C, react for 5h, then raise the temperature to 135°C, react for 2h, cool and discharge to obtain double-ended epoxy silicone oil.

[0025] Example 1

[0026] (1) adding a polymerization inhibitor, butylated hydroxytoluene, a tetrahydrofuran solution of chloroplatinic acid, and acrylic acid to an N,N-dimethylformamide solvent, stirring evenly, and then adding silicone rubber, wherein the mass ratio of the polymerization inhibitor, butylated hydroxytoluene, the catalyst, chloroplatinic acid, acrylic acid, and silicone rubber is 0.01:0.02:1:1.1, ultrasonically dispersing evenly, reacting at 65° C. for 6 hours, cooling after completion, centrifuging, washing, and drying to obtain a carboxylated silicone rubber;

[0027] (2) adding diethanolamine and double-ended epoxy silicone oil into a reactor filled with isopropanol solvent, wherein the mass ratio of diethanolamine to double-ended epoxy silicone oil is 1.5:1, reacting at 55° C. for 14 h, concentrating after completion, and washing with methanol to obtain intermediate 1;

[0028] (3) adding intermediate 1 and carboxylated silicone rubber to N,N-dimethylformamide solvent, stirring evenly, and then continuing to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, carboxylated silicone rubber, and p-toluenesulfonic acid catalyst is 1:1.2:0.02, reacting at 80° C. for 5 h, and then distilling under reduced pressure after the reaction, filtering and drying to obtain intermediate 2;

[0029] (4) adding 10 parts by weight of octadecane chloride and 8 parts by weight of intermediate 2 into N,N-dimethylformamide solvent, reacting at 85° C. for 4 hours, concentrating after the reaction, and washing with methanol to obtain modified silicone rubber;

[0030] (5) 5 parts by weight of intermediate 1, 1 part by weight of pyridine, and 7 parts by weight of p-methoxybenzoyl chloride were added to a dichloromethane solvent at -5°C, and then reacted at 25°C for 8 hours, the solvent was concentrated, and the filter cake was washed to obtain intermediate 3;

[0031] (6) 10 parts by weight of the intermediate 3 was added to a dichloromethane solvent, 0.8 parts by weight of boron tribromide was added dropwise at -23°C, the reaction was allowed to proceed for 15 hours, and then 5 parts by weight of methanol was added dropwise to terminate the reaction. The solution was poured into ice water to precipitate, filtered, the filter cake was washed, and recrystallized to obtain phenolic silane;

[0032] (7) adding 7 parts by weight of phenolic silane, 10 parts by weight of phenol, and 18 parts by weight of a 38% formaldehyde aqueous solution to a reactor, stirring evenly, adding 0.9 parts by weight of a catalyst oxalic acid, reacting at 60° C. for 5 h, standing to separate, filtering, washing with water, and drying to obtain a modified phenolic resin;

[0033] (8) 8 parts by weight of modified silicone rubber, 6 parts by weight of modified phenolic resin, 2 parts by weight of talc, 1 part by weight of dipropylene glycol butyl ether film-forming aid, 0.2 parts by weight of polysiloxane defoaming agent, 0.4 parts by weight of ammonium acrylate wetting agent, and 12 parts by weight of water are mixed and stirred, and after stirring evenly, allowed to stand at room temperature for 3 hours to obtain a waterproof coating containing modified silicone rubber.

[0034] Example 2

[0035] (1) adding a polymerization inhibitor, butylated hydroxytoluene, a tetrahydrofuran solution of chloroplatinic acid, and acrylic acid to an N,N-dimethylformamide solvent, stirring evenly, and then adding silicone rubber, wherein the mass ratio of the polymerization inhibitor, butylated hydroxytoluene, the catalyst, chloroplatinic acid, acrylic acid, and silicone rubber is 0.03:0.03:1:1.3, ultrasonically dispersing evenly, reacting at 80° C. for 10 hours, cooling after completion, centrifuging, washing, and drying to obtain a carboxylated silicone rubber;

[0036] (2) adding diethanolamine and double-ended epoxy silicone oil into a reactor filled with isopropanol solvent, wherein the mass ratio of diethanolamine to double-ended epoxy silicone oil is 2.2:1, reacting at 70° C. for 18 h, concentrating after completion, and washing with methanol to obtain intermediate 1;

[0037] (3) adding intermediate 1 and carboxylated silicone rubber to N,N-dimethylformamide solvent, stirring evenly, and then continuing to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, carboxylated silicone rubber, and p-toluenesulfonic acid catalyst is 1:1.4:0.04, reacting at 95° C. for 8 h, and then distilling under reduced pressure after the reaction, filtering and drying to obtain intermediate 2;

[0038] (4) adding 12 parts by weight of octadecane chloride and 15 parts by weight of intermediate 2 into N,N-dimethylformamide solvent, reacting at 100° C. for 7 h, concentrating after the reaction, and washing with methanol to obtain modified silicone rubber;

[0039] (5) 8 parts by weight of intermediate 1, 1.5 parts by weight of pyridine, and 10 parts by weight of p-methoxybenzoyl chloride were added to a dichloromethane solvent at -2°C, and then reacted at 40°C for 14 hours, the solvent was concentrated, and the filter cake was washed to obtain intermediate 3;

[0040] (6) 13 parts by weight of the intermediate 3 was added to a dichloromethane solvent, 1.4 parts by weight of boron tribromide was added dropwise at -10°C, the reaction was allowed to proceed for 20 hours, and then 7 parts by weight of methanol was added dropwise to terminate the reaction. The solution was poured into ice water to precipitate, filtered, the filter cake was washed, and recrystallized to obtain phenolic silane;

[0041] (7) adding 12 parts by weight of phenolic silane, 16 parts by weight of phenol, and 30 parts by weight of a 41% formaldehyde aqueous solution to a reactor, stirring evenly, adding 1.2 parts by weight of a catalyst oxalic acid, reacting at 85° C. for 9 hours, standing to separate, filtering, washing with water, and drying to obtain a modified phenolic resin;

[0042] (8) 12 parts by weight of modified silicone rubber, 10 parts by weight of modified phenolic resin, 3 parts by weight of talc, 2 parts by weight of dipropylene glycol butyl ether film-forming aid, 0.5 parts by weight of polysiloxane defoaming agent, 0.7 parts by weight of ammonium acrylate wetting agent, and 16 parts by weight of water are mixed and stirred, and after stirring evenly, the mixture is allowed to stand at room temperature for 4 hours to obtain a waterproof coating containing modified silicone rubber.

[0043] Example 3

[0044] (1) adding a polymerization inhibitor, butylated hydroxytoluene, a tetrahydrofuran solution of chloroplatinic acid, and acrylic acid to an N,N-dimethylformamide solvent, stirring evenly, and then adding silicone rubber, wherein the mass ratio of the polymerization inhibitor, butylated hydroxytoluene, the catalyst, chloroplatinic acid, acrylic acid, and silicone rubber is 0.02:0.025:1:1.2, ultrasonically dispersing evenly, reacting at 72.5° C. for 8 hours, cooling after completion, centrifuging, washing, and drying to obtain a carboxylated silicone rubber;

[0045] (2) adding diethanolamine and double-ended epoxy silicone oil into a reactor filled with isopropanol solvent, wherein the mass ratio of diethanolamine to double-ended epoxy silicone oil is 1.85:1, reacting at 62.5° C. for 16 h, concentrating after completion, and washing with methanol to obtain intermediate 1;

[0046] (3) adding intermediate 1 and carboxylated silicone rubber to N,N-dimethylformamide solvent, stirring evenly, and then continuing to add p-toluenesulfonic acid catalyst, wherein the mass ratio of intermediate 1, carboxylated silicone rubber, and p-toluenesulfonic acid catalyst is 1:1.3:0.03, reacting at 87.5°C for 6.5h, and then performing reduced pressure distillation after completion, filtering and drying to obtain intermediate 2;

[0047] (4) adding 11 parts by weight of octadecane chloride and 11.5 parts by weight of intermediate 2 to N,N-dimethylformamide solvent, reacting at 92.5° C. for 5.5 hours, concentrating after the reaction, and washing with methanol to obtain modified silicone rubber;

[0048] (5) 6.5 parts by weight of intermediate 1, 1.25 parts by weight of pyridine, and 8.5 parts by weight of p-methoxybenzoyl chloride were added to a dichloromethane solvent at -3.5°C, and then reacted at 32.5°C for 11 hours, the solvent was concentrated, and the filter cake was washed to obtain intermediate 3;

[0049] (6) 11.5 parts by weight of the intermediate 3 was added to a dichloromethane solvent, 1.1 parts by weight of boron tribromide was added dropwise at -16.5°C, the reaction was continued for 17.5 hours, and then 67 parts by weight of methanol was added dropwise to terminate the reaction. The solution was poured into ice water to precipitate, filtered, the filter cake was washed, and recrystallized to obtain phenolic silane;

[0050] (7) adding 9.5 parts by weight of phenolic silane, 13 parts by weight of phenol, and 24 parts by weight of a 39.5% formaldehyde aqueous solution to a reactor, stirring evenly, adding 1.05 parts by weight of oxalic acid as a catalyst, reacting at 72.5° C. for 7 h, standing to separate, filtering, washing with water, and drying to obtain a modified phenolic resin;

[0051] (8) 10 parts by weight of modified silicone rubber, 8 parts by weight of modified phenolic resin, 2.5 parts by weight of talc, 1.5 parts by weight of dipropylene glycol butyl ether film-forming aid, 0.35 parts by weight of polysiloxane defoaming agent, 0.55 parts by weight of ammonium acrylate wetting agent, and 14 parts by weight of water are mixed and stirred, and after stirring evenly, the mixture is allowed to stand at room temperature for 3.5 hours to obtain a waterproof coating containing modified silicone rubber.

[0052] Comparative Example 1

[0053] (1) 8 parts by weight of a modified phenolic resin, 2.5 parts by weight of talc, 1.5 parts by weight of a dipropylene glycol butyl ether film-forming aid, 0.35 parts by weight of a polysiloxane defoamer, 0.55 parts by weight of an acrylic acid ammonium salt wetting agent, and 14 parts by weight of water are mixed and stirred, and after being stirred evenly, the mixture is allowed to stand at room temperature for 3.5 hours to obtain a waterproof coating containing modified silicone rubber.

[0054] Comparative Example 2

[0055] (8) 10 parts by weight of modified silicone rubber, 2.5 parts by weight of talc, 1.5 parts by weight of dipropylene glycol butyl ether film-forming aid, 0.35 parts by weight of polysiloxane defoaming agent, 0.55 parts by weight of ammonium acrylate wetting agent, and 14 parts by weight of water are mixed and stirred, and after stirring evenly, the mixture is allowed to stand at room temperature for 3.5 hours to obtain a waterproof coating containing modified silicone rubber.

[0056] The water resistance of waterproof coatings was tested according to the method in GB / T16777-2008 "Test Methods for Building Waterproof Coatings". The prepared specimens were weighed, immersed in 20±2℃ water for 24h, taken out and quickly wiped off the free moisture on the surface of the specimens, and weighed again to calculate the water absorption rate. The test results are shown in Table 1.

[0057] Table 1: Coating waterproof test.

[0058]

[0059]

[0060] It can be seen from Table 1 that Examples 1-3 of the present invention have lower water absorption rates than Comparative Examples 1-2, indicating better waterproofing effects.

[0061] Antibacterial performance: Carefully tear off the coating and cut it into a 10mm diameter disc, sterilize it with a UV lamp, add it to 10mL solid agar medium and culture it with Staphylococcus aureus (10μL, 106CFU / mL) in a 37℃ incubator for 12 hours. The experiment uses three groups of parallel controls and takes the average value. The blank control is carried out without the coating, and then the CFU count is determined. The calculation formula of the antibacterial rate is shown as follows: Antibacterial rate (%) = (1-C / N) × 100%. Among them, N is the average number of live bacteria in the blank control group after 12h, and C is the average number of live bacteria in the experimental group after 12h. The test results are shown in Table 2.

[0062] Table 2: Antibacterial rate test.

[0063] project Antibacterial rate (%) Example 1 96 Example 2 99 Example 3 98 Comparative Example 1 83 Comparative Example 2 72

[0064] It can be seen from Table 2 that Examples 1-3 of the present invention have better antibacterial properties than Comparative Examples 1-2.

[0065] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A waterproof coating containing modified silicone rubber, characterized in that: The invention comprises the following components by weight: 8-12 parts by weight of modified silicone rubber, 6-10 parts by weight of modified phenolic resin, 2-3 parts by weight of talc, 1-2 parts by weight of dipropylene glycol butyl ether film-forming aid, 0.2-0.5 parts by weight of polysiloxane defoamer, 0.4-0.7 parts by weight of ammonium acrylate wetting agent, and 12-16 parts by weight of water; The preparation method of the modified silicone rubber is: (1) Adding a polymerization inhibitor, butylated hydroxytoluene, a tetrahydrofuran solution of chloroplatinic acid, and acrylic acid to an N,N-dimethylformamide solvent, stirring evenly, then adding silicone rubber, dispersing evenly by ultrasonication, reacting at 65-80°C for 6-10h, cooling after reaction, centrifuging, washing, and drying to obtain a carboxylated silicone rubber; (2) Add diethanolamine and double-ended epoxy silicone oil into a reactor filled with isopropanol solvent, react at 55-70°C for 14-18 hours, concentrate and wash with methanol to obtain intermediate 1; (3) Add intermediate 1 and carboxylated silicone rubber to N,N-dimethylformamide solvent, stir evenly, then continue to add p-toluenesulfonic acid catalyst, react at 80-95°C for 5-8h, and then distill under reduced pressure, filter and dry to obtain intermediate 2; (4) adding 10-12 parts by weight of octadecane chloride and 8-15 parts by weight of intermediate 2 into N,N-dimethylformamide solvent, reacting at 85-100° C. for 4-7 hours, concentrating after the reaction, and washing with methanol to obtain modified silicone rubber; The mass ratio of the polymerization inhibitor dibutyl hydroxytoluene, the catalyst chloroplatinic acid, acrylic acid, and the silicone rubber in (1) is 0.01-0.03:0.02-0.03:1:1.1-1.3; The mass ratio of diethanolamine to double-terminal epoxy silicone oil in (2) is 1.5-2.2:1; The mass ratio of the intermediate 1, carboxylated silicone rubber and p-toluenesulfonic acid catalyst in (3) is 1:1.2-1.4:0.02-0.04; The preparation method of the modified phenolic resin is: S1. 5-8 parts by weight of intermediate 1, 1-1.5 parts by weight of pyridine, and 7-10 parts by weight of p-methoxybenzoyl chloride are added to a dichloromethane solvent at -5°C to -2°C, and then reacted at 25-40°C for 8-14h, the solvent is concentrated, and the filter cake is washed to obtain intermediate 3; S2. 10-13 parts by weight of intermediate 3 is added to a dichloromethane solvent, 0.8-1.4 parts by weight of boron tribromide is added dropwise at -23°C to -10°C, the reaction is continued for 15-20 hours, and then 5-7 parts by weight of methanol are added dropwise to terminate the reaction, the solution is poured into ice water to precipitate, filtered, the filter cake is washed, and recrystallized to obtain phenolic silane; S3. 7-12 parts by weight of phenolic silane, 10-16 parts by weight of phenol, 18-30 parts by weight of formaldehyde solution were added to the reactor, stirred and then 0.9-1.2 parts by weight of oxalic acid catalyst was added, and the reaction was carried out at 60-85 ° C for 5-9h, and after the reaction, the mixture was allowed to stand for stratification, filtered, washed with water and dried to obtain a modified phenolic resin; The mass fraction of the aqueous solution of formaldehyde in S3 is 38-41%.

2. A method for preparing a waterproof coating containing modified silicone rubber as claimed in claim 1, characterized in that: The preparation method of the waterproof coating containing modified silicone rubber comprises the following steps: mixing and stirring the modified silicone rubber, modified phenolic resin, talcum powder, dipropylene glycol butyl ether film-forming aid, polysiloxane defoamer, ammonium acrylate wetting agent and water, stirring evenly, and standing at room temperature for 3-4 hours to obtain the waterproof coating containing modified silicone rubber.