Wafer bonding film, memory chip and preparation method thereof
By adjusting the proportion of epoxy resin and adding materials such as silica, the prepared wafer bonding film solves the problem of bubble control in chip packaging, improves packaging yield, and achieves high adhesion and low modulus.
Patent Information
- Application Number
- CN202411073960.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-07
AI Technical Summary
During the chip packaging process, it is difficult to control the bubbles in large-size chips, which leads to the formation of voids after curing and affects the packaging yield.
By adjusting the ratio of rubber-modified epoxy resin, acrylic epoxy resin, flexible epoxy resin and polyurethane-modified epoxy resin, and combining silica, phenolic curing agent and accelerator, a wafer bonding film is prepared to reduce the Storage modulus and water absorption, thereby improving the chip packaging yield.
It achieves high adhesion and low modulus of the wafer bonding film, reduces internal stress and thermal expansion coefficient, allows it to closely contact the chip at high temperatures, eliminates bubbles, and improves packaging yield.
Smart Images

Figure CN118599460B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chip packaging, and in particular relates to a wafer bonding film, a memory chip and a preparation method thereof. Background Art
[0002] Wafer adhesive film is a key material commonly used in the chip packaging process. Wafer adhesive film is used during laser cutting in the chip packaging process. Wafers can be cut and separated together and peeled off so that the wafers after cutting are still adhered to the film and will not be scattered due to cutting. At the same time, both sides of the wafer adhesive film can be bonded to chips or substrates to achieve multi-chip packaging. At present, bubbles are difficult to control when bonding large-sized chips, and voids are easily formed after curing, which in turn affects the chip packaging yield.
[0003] Therefore, how to provide a chip bonding film, reduce the storage modulus and water absorption of the chip bonding film by adjusting the ratio between rubber-modified epoxy resin, acrylic epoxy resin, flexible epoxy resin and polyurethane-modified epoxy resin, and thus improve the chip packaging yield, is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0004] The object of the present invention is to provide a wafer bonding film, a memory chip and a method for preparing the same, so as to solve at least one of the above-mentioned technical problems.
[0005] To achieve the above-mentioned purpose, the first aspect of the present invention provides a wafer bonding film, which comprises the following components by mass: 20 to 30 parts of silicon dioxide, 20 to 25 parts of rubber-modified epoxy resin, 10 to 15 parts of acrylic epoxy resin, 10 to 20 parts of flexible epoxy resin, 15 to 20 parts of polyurethane-modified epoxy resin, 20 to 25 parts of curing agent, and 0.5 to 1.0 part of accelerator; the flexible epoxy resin is YX-7400.
[0006] In the first aspect, the silica is spherical silica, and the particle size D50 of the spherical silica is 0.6 μm.
[0007] In the first aspect, the curing agent is a phenolic curing agent; the phenolic curing agent includes a liquid curing agent and a solid curing agent.
[0008] In the first aspect, the liquid curing agent is MTH-8000; the solid curing agent is YLOK aralkylphenol resin.
[0009] In the first aspect, the accelerator is an imidazole compound.
[0010] In the first aspect, the rubber-modified epoxy resin is HyPox RK84L.
[0011] In the first aspect, the polyurethane-modified epoxy resin is EPU-133.
[0012] A second aspect of the present invention provides a method for preparing the wafer bonding film as described in the first aspect, the preparation method comprising:
[0013] S1. Stir and mix the components according to their respective mass fractions to obtain a first slurry; the mass fractions of the components specifically include: 20-30 parts of silicon dioxide, 20-25 parts of rubber-modified epoxy resin, 10-15 parts of acrylic epoxy resin, 10-20 parts of flexible epoxy resin, 15-20 parts of polyurethane-modified epoxy resin, 20-25 parts of curing agent, and 0.5-1.0 parts of accelerator; the flexible epoxy resin is YX-7400;
[0014] S2, transferring the first slurry to a bead mill for grinding to obtain a uniform second slurry;
[0015] S3, vacuum degassing the second slurry to obtain a third slurry;
[0016] S4, the third slurry is coated by a coating machine and baked;
[0017] S5. After baking, a wafer bonding film is obtained.
[0018] The third aspect of the present invention provides a method for preparing a memory chip, the preparation method comprising: obtaining a memory chip body; attaching a wafer adhesive film to the surface of the memory chip body to obtain a pre-packaged chip; the wafer adhesive film is made by the wafer adhesive film preparation method described in the second aspect; cutting, chip bonding, and wire bonding the pre-packaged chip to obtain a chip as a whole; pressurizing and curing the chip as a whole to obtain a well-packaged memory chip; the pressurizing and curing conditions include: pressure of 0.8MPa, temperature of 175°C, and time of 4h.
[0019] A fourth aspect of the present invention provides a memory chip, which is manufactured using the memory chip manufacturing method described in the third aspect.
[0020] Beneficial Effects
[0021] The present invention provides a wafer bonding film, which comprises the following components by mass: 20 to 30 parts of silicon dioxide, 20 to 25 parts of rubber-modified epoxy resin, 10 to 15 parts of acrylic epoxy resin, 10 to 20 parts of flexible epoxy resin, 15 to 20 parts of polyurethane-modified epoxy resin, 20 to 25 parts of curing agent, and 0.5 to 1.0 parts of accelerator; the flexible epoxy resin is YX-7400; the film-forming property of the rubber-modified epoxy resin, the water absorption property of the acrylic epoxy resin, and the flexible epoxy resin are used to form a wafer bonding film. The resilience of epoxy resin and the adhesion of polyurethane modified epoxy resin are combined, and the ratio between the four is adjusted to form a mixed epoxy resin. Under the action of the accelerator, the curing agent and the mixed epoxy resin are cross-linked to form a whole, so that the wafer bonding film has higher adhesion and low modulus. At the same time, silicon dioxide is used to reduce the internal stress and thermal expansion coefficient of the wafer bonding film, so that during the chip packaging process, the wafer bonding film is in a molten state at high temperature and can be in close contact with the chip, thereby improving the chip packaging yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 The present invention is a flow chart of a method for preparing a wafer bonding film. DETAILED DESCRIPTION
[0024] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.
[0025] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. In the event of a conflict, the present specification takes precedence.
[0026] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or obtained by existing methods.
[0027] The present application provides a wafer bonding film, which comprises the following components by mass: 20 to 30 parts of silicon dioxide, 20 to 25 parts of rubber-modified epoxy resin, 10 to 15 parts of acrylic epoxy resin, 10 to 20 parts of flexible epoxy resin, 15 to 20 parts of polyurethane-modified epoxy resin, 20 to 25 parts of curing agent, and 0.5 to 1.0 part of accelerator; the flexible epoxy resin is YX-7400.
[0028] Specifically, the present invention provides a wafer bonding film, which comprises the following components by mass: 20 to 30 parts of silicon dioxide, 20 to 25 parts of rubber-modified epoxy resin, 10 to 15 parts of acrylic epoxy resin, 10 to 20 parts of flexible epoxy resin, 15 to 20 parts of polyurethane-modified epoxy resin, 20 to 25 parts of curing agent, and 0.5 to 1.0 parts of accelerator; the flexible epoxy resin is YX-7400; the film-forming property of the rubber-modified epoxy resin, the water absorption property of the acrylic epoxy resin, The resilience of the flexible epoxy resin and the adhesion of the polyurethane modified epoxy resin are used to adjust the ratio between the four to form a mixed epoxy resin. Under the action of the accelerator, the curing agent and the mixed epoxy resin are cross-linked to form a whole, so that the chip bonding film has higher adhesion and low modulus. At the same time, silicon dioxide is used to reduce the internal stress and thermal expansion coefficient of the chip bonding film, so that during the chip packaging process, the chip bonding film is in a molten state at high temperature and can be in close contact with the chip, thereby improving the chip packaging yield.
[0029] In some possible embodiments, the silicon dioxide is spherical silicon dioxide, and the particle size D50 of the spherical silicon dioxide is 0.6 μm.
[0030] This is because the use of spherical silica as a filling material can avoid agglomeration during the melting process, which in turn affects the fluidity of the wafer bonding film glue in the molten state. It can also adjust the storage modulus and thermal expansion coefficient of the wafer bonding film and improve the chip packaging yield.
[0031] In some possible embodiments, the curing agent is a phenolic curing agent; the phenolic curing agent includes a liquid curing agent and a solid curing agent.
[0032] In some possible embodiments, the liquid curing agent is MTH-8000; the solid curing agent is YLOK aralkylphenol resin.
[0033] Those skilled in the art can understand that the present application uses YLOK aralkylphenol resin as a solid curing agent, which can not only react with epoxy resin, but also improve the adhesion of the wafer bonding film. Furthermore, using MTH-8000 as a liquid curing agent can increase the contact area with the epoxy resin, and by adjusting the ratio of the solid curing agent to the liquid curing agent, the reaction efficiency of the wafer bonding film during the melting and curing process can be controlled.
[0034] In some possible embodiments, the promoter is an imidazole compound.
[0035] At a certain temperature, the accelerator can speed up the reaction rate of epoxy resin and curing agent, reduce the curing time and improve production efficiency.
[0036] In some possible embodiments, the rubber modified epoxy resin is HyPox RK84L.
[0037] The epoxy equivalent of HyPox RK84L epoxy resin is 1250-1500 g / eq, with high toughness and elasticity. By adjusting the proportion of HyPox RK84L, the tensile strength of the wafer bonding film can be controlled.
[0038] In some possible embodiments, the polyurethane-modified epoxy resin is EPU-133.
[0039] The epoxy equivalent of the polyurethane modified epoxy resin EPU-133 is 230 g / eq. By adjusting the proportion of EPU-133, the viscosity of the wafer adhesive film can be adjusted, and the adhesion between the wafer adhesive film and the chip can be improved, thereby improving the chip packaging yield.
[0040] Based on a general inventive concept, see Figure 1 The present application also provides a method for preparing the wafer bonding film as described in the first aspect, the preparation method comprising:
[0041] S1. Stir and mix the components according to their respective mass fractions to obtain a first slurry; the mass fractions of the components specifically include: 20-30 parts of silicon dioxide, 20-25 parts of rubber-modified epoxy resin, 10-15 parts of acrylic epoxy resin, 10-20 parts of flexible epoxy resin, 15-20 parts of polyurethane-modified epoxy resin, 20-25 parts of curing agent, and 0.5-1.0 parts of accelerator; the flexible epoxy resin is YX-7400;
[0042] S2, transferring the first slurry to a bead mill for grinding to obtain a uniform second slurry;
[0043] S3, vacuum degassing the second slurry to obtain a third slurry;
[0044] S4, the third slurry is coated by a coating machine and baked;
[0045] S5. After baking, a wafer bonding film is obtained.
[0046] The preparation method of the wafer bonding film provided in the present application is simple and easy to operate. The slurry after coating is baked in a programmed temperature manner to remove the solvent, thereby obtaining a wafer bonding film with uniform thickness and no holes.
[0047] Based on a general inventive concept, a method for preparing a memory chip comprises:
[0048] (1) Obtain the memory chip body;
[0049] (2) affixing a wafer adhesive film to the surface of the memory chip body to obtain a pre-packaged chip; the wafer adhesive film is made by the method for preparing a wafer adhesive film according to the second aspect;
[0050] (3) cutting, chip bonding, and wire bonding the pre-packaged chip to obtain a whole chip;
[0051] (4) Pressurizing and curing the entire chip to obtain a well-packaged memory chip; the pressurizing and curing conditions include: pressure of 0.8 MPa, temperature of 175° C., and time of 4 hours.
[0052] Those skilled in the art will understand that the wafer adhesive film prepared according to the formula ratio in the first aspect has a certain degree of adhesion, can be attached to the surface of the chip body, and the chip body is preliminarily packaged. Then, through cutting, chip bonding and wire bonding, a chip of suitable size is obtained as a whole. The chip as a whole is pressurized and cured under the conditions of a pressure of 0.8 MPa and a temperature of 175°C, so that the wafer adhesive film is in a molten state under these conditions, so as to discharge the bubbles between the wafer adhesive film and the chip. After 4 hours, the pressure and temperature are removed to obtain a well-packaged memory chip.
[0053] Based on a general inventive concept, the present application also provides a memory chip, which is manufactured using the memory chip manufacturing method described in the third aspect.
[0054] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0055] The components of the raw materials in Comparative Examples 1-9 and Examples 1-7 are shown in Table 1-2 below according to their mass fractions:
[0056] Table 1 Distribution ratio of each group of raw materials in the comparative example
[0057]
[0058] Table 2 Distribution ratio of each group of raw materials in the embodiment
[0059]
[0060] The wafer adhesive films provided in Examples 1-7 and Comparative Examples 1-9 were tested for storage modulus, temperature rise / constant temperature rheology, moisture absorption rate, and silicon wafer adhesion after curing. The specific test process is as follows:
[0061] 1. Storage modulus test after curing: Reference standard: ASTM E2254-2018, take a sample that is completely cured at 175℃ / 1h, prepare a test sample with a size of 25mm×6.5mm×0.25mm, measurement mode: Tension: Film, heat up to 250℃ at 5℃ / min, and take the storage modulus at 25℃ and 200℃;
[0062] 2. Temperature Rheology Test: The sample is made into a disc with a thickness of 1mm and a diameter of 20mm. Test mode: Oscillation Temperature Ramp, heating program: 25℃ to 200℃, heating rate: 5℃ / min;
[0063] 3. Constant temperature rheological test: The sample is made into a disc with a thickness of 1mm and a diameter of 20mm. Test mode: Oscillation Temperature Ramp, program: 25℃ to 165℃, then keep constant temperature at 165℃ for 4 hours, heating rate: 5℃ / min;
[0064] 4. Moisture absorption test: Take a 50mm×50mm film and transfer it to a silicon wafer. After curing at 175℃ for 1 hour, weigh it. Then immerse the silicon wafer vertically and completely in a glass container filled with 25±1℃ distilled water. There should be no bubbles on the surface and it should not touch the container wall. After immersion for 24 hours, take it out with tweezers, quickly dry the surface moisture of the membrane with filter paper, and weigh it immediately.
[0065] 5. Silicon wafer adhesion: Transfer a 2mm×2mm film with a thickness of 25μm to a 10mm×10mm silicon wafer, then cover it with a 2mm×2mm silicon wafer and clamp it with a clip. After curing at 175℃ for 1h, use a multi-function shear force tester to test the shear bonding strength at 25℃ and 260℃.
[0066] The test results are shown in Table 3 below:
[0067] Table 3 Test results
[0068]
[0069] It can be seen from the above table that adding acrylic epoxy resin to the wafer adhesive film has lower water absorption and storage modulus; the wafer adhesive film prepared by using YX-7400 flexible epoxy resin has lower storage modulus and higher silicon wafer adhesion. The wafer adhesive film prepared according to the formula ratio of this application has ultra-low storage modulus, low moisture absorption rate and high silicon wafer adhesion; during the temperature rise curing process, the rheological viscosity of the wafer adhesive film gradually increases, and through the data of the temperature rise rheological viscosity and the constant temperature rheological viscosity, it can be seen that the rheological viscosity change gap of the wafer adhesive film prepared by using Examples 1-7 is smaller than that of the film prepared by using Comparative Examples 1-9. It can be understood that the wafer adhesive film of this application has better stability. The baked wafer adhesive film is attached to the surface of the chip, and it is cut, chip bonded, wire bonded, and pressurized and cured, so that the wafer adhesive film is in a molten state at high temperature, so as to discharge the bubbles between the chip and the wafer adhesive film, thereby improving the chip packaging yield.
[0070] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.
[0071] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0072] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A wafer bonding film, characterized in that: The wafer bonding film comprises the following components by weight: 20-30 parts of silicon dioxide, 20-25 parts of rubber-modified epoxy resin, 10-15 parts of acrylic epoxy resin, 10-20 parts of flexible epoxy resin, 15-20 parts of polyurethane-modified epoxy resin, 20-25 parts of curing agent, and 0.5-1.0 parts of accelerator; the flexible epoxy resin is YX-7400; The curing agent is a phenolic curing agent; the phenolic curing agent includes a liquid curing agent and a solid curing agent; The liquid curing agent is MTH-8000; the solid curing agent is YLOK aralkylphenol resin; The rubber modified epoxy resin is HyPox RK84L; The polyurethane modified epoxy resin is EPU-133.
2. The wafer bonding film according to claim 1, wherein: The silicon dioxide is spherical silicon dioxide, and the particle size D50 of the spherical silicon dioxide is 0.6 μm.
3. The wafer bonding film according to claim 2, characterized in that: The accelerator is an imidazole compound.
4. A method for preparing a wafer bonding film according to any one of claims 1 to 3, characterized in that: The preparation method comprises: S1. Stir and mix the components according to their respective mass fractions to obtain a first slurry; the mass fractions of the components specifically include: 20-30 parts of silicon dioxide, 20-25 parts of rubber-modified epoxy resin, 10-15 parts of acrylic epoxy resin, 10-20 parts of flexible epoxy resin, 15-20 parts of polyurethane-modified epoxy resin, 20-25 parts of curing agent, and 0.5-1.0 parts of accelerator; the flexible epoxy resin is YX-7400; S2, transferring the first slurry to a bead mill for grinding to obtain a uniform second slurry; S3, vacuum degassing the second slurry to obtain a third slurry; S4, the third slurry is coated by a coating machine and baked; S5. After baking, a wafer bonding film is obtained.
5. A method for preparing a memory chip, characterized in that: The preparation method comprises: Get the memory chip body; A wafer adhesive film is attached to the surface of the memory chip body to obtain a pre-packaged chip; the wafer adhesive film is made by the method for preparing a wafer adhesive film according to claim 4; Cutting, chip bonding, and wire bonding the pre-packaged chip to obtain a whole chip; The chip is pressurized and cured as a whole to obtain a well-packaged memory chip; the pressurized curing conditions include: a pressure of 0.8 MPa, a temperature of 175° C., and a time of 4 hours.
6. A memory chip, characterized in that: The memory chip is manufactured by the memory chip manufacturing method according to claim 5.
Citation Information
Patent Citations
Resin composition, cured product of resin composition, resin sheet, printed wiring board, semiconductor chip package, and semiconductor device
CN113462276A
Underfill adhesive with low thermal expansion coefficient, preparation method thereof and chip packaging structure
CN117801745A