A sodium ion battery positive electrode active material and preparation method thereof
By using ultrasonic stirring and microwave heating in the positive electrode material of sodium ion battery, the surface modification layer and doping structure are formed, which solves the stability problem of the material during the charging and discharging process, improves the electrochemical performance and cycle stability, and extends the Battery life.
Patent Information
- Application Number
- CN202411118249.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing sodium ion battery positive electrode materials are prone to multi-stage phase change, lattice distortion and poor chemical stability during charging and discharging, resulting in reduced cycling performance and difficult to regulate the crystal structure of the material in the preparation process, affecting the stability and life of the battery.
Sodium carbonate, titanium sulfate, phosphate and NaNi0.5Mn0.5O2 were used to ultrasonic stir in ethylene glycol and microwave heating, and two heat treatments were carried out to form a surface modification layer and doped structure, adjust the crystal structure and uniformity of the material, and improve the Electrochemical properties and air stability.
Through surface regulation modification and ion doping, the electrochemical performance and air stability of the material are enhanced, irreversible phase change and lattice distortion are suppressed, cycle stability and battery performance are improved, and battery life is extended.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion batteries, and in particular to a sodium ion battery positive electrode active material and a preparation method thereof. Background Art
[0002] Due to the shortage of lithium resources and the increasing cost, sodium-ion batteries have greatly reduced costs due to the high abundance and high energy density of sodium, and sodium does not react with aluminum to form alloys. Therefore, sodium-ion batteries have become a powerful alternative to lithium-ion batteries. In terms of safety, sodium is the next element in the lithium cycle and has more stable chemical properties. In addition, the internal resistance of sodium-ion batteries is higher than that of lithium-ion batteries, which results in less heat accumulation immediately under insufficient power. In recent years, sodium-ion battery cathode materials have been widely studied, such as layered oxides, polyanionic compounds, and Prussian blue and its analogs.
[0003] Among them, layered oxides (NaNi 0.5 Mn 0.5 O2) has attracted wide attention due to its high electrochemical activity, high theoretical specific capacity and easy synthesis. However, some problems may arise in actual production applications, such as NaNi 0.5 Mn 0.5 O2 materials undergo multi-level phase transitions during the charge and discharge process. 3+ and Ni 2+ The Jahn-Teller effect (Jiang Taylor effect) is a lattice distortion that easily occurs during the sodium ion insertion and extraction process, causing an irreversible phase transition, which greatly reduces the cycle performance of the material. In addition, the layered oxide NaNi 0.5 Mn 0.5 O2 materials have poor chemical stability when exposed to air. The main reasons for this phenomenon are: ① Synthesis of NaNi 0.5 Mn 0.5 O2 material, due to excessive sodium in local areas or side reactions, Na2O2 impurities are generated at the interface. Na2O2 is easy to react with electrolyte to generate impurities such as Na2CO3 and NaOH; ②NaNi 0.5 Mn 0.5 O2 materials can also react chemically with CO2 and H2O in the air to generate impurities such as Na2CO3 and NaOH. The impurities generated in these situations directly reduce the electrochemical performance of the material.
[0004] In addition, the current preparation process of positive electrode materials for sodium-ion batteries generally involves mixing various metal raw materials or precursors and directly sintering them at high temperatures. Although the preparation method is simple, it is difficult to control the crystal structure of the material, resulting in unevenness, cracking and dissolution of transition metal ions, affecting the stability and charge and discharge performance of the battery, and affecting the battery life. Summary of the invention
[0005] In view of this, the present invention proposes a sodium ion battery positive electrode active material and a preparation method thereof to solve the above problems.
[0006] The technical solution of the present invention is achieved in this way:
[0007] A method for preparing a positive electrode active material for a sodium ion battery, the specific steps comprising:
[0008] (1) Sodium carbonate, titanium sulfate, phosphate and NaNi 0.5 Mn 0.5 O2 is added to ethylene glycol, ultrasonically stirred, assisted by microwave heating, washed, filtered, and dried to obtain a mixture;
[0009] The sodium carbonate, titanium sulfate, phosphate and NaNi 0.5 Mn 0.5 The molar ratio of O2 is 1:(2.1-2.3):7:(1.03-1.05);
[0010] The phosphate is composed of sodium phosphate and ammonium dihydrogen phosphate in a molar ratio of 3:4;
[0011] (2) The mixture is heat-treated twice under an inert atmosphere to obtain the target sodium ion battery positive electrode active material.
[0012] Further, in step (1), the NaNi 0.5 Mn 0.5 O2 is prepared by high temperature solid phase method, coprecipitation method or sol-gel method.
[0013] Further, in step (1), the ethylene glycol and NaNi 0.5 Mn 0.5 The liquid-to-solid ratio of O2 is 50-60:1mL / g.
[0014] Furthermore, in step (1), the ultrasonic stirring time is 1.5-2.5h, the rotation speed is 300-400rpm, the power is 200-300W, and the temperature is 30-40°C.
[0015] Furthermore, in step (1), the microwave heating is carried out at 400-500 W and 40-50° C. for 30-60 min.
[0016] Furthermore, in step (2), the two heat treatments are as follows: first, the temperature is raised to 300-400°C at a heating rate of 3°C / min for 4.5-5.5h, and then the temperature is raised to 650-750°C at a heating rate of 1°C / min for 5.5-6.5h.
[0017] A sodium ion battery positive electrode active material is prepared by any one of the preparation methods described above.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The present invention uses surface modification and ion doping to treat layered oxides (NaNi 0.5 Mn 0.5 O2) materials are synergistically modified to clarify the intrinsic mechanism of surface regulation modification and ion doping to enhance the air stability and ion transfer rate of the material. The two together improve the electrochemical performance and air stability of the positive electrode material. The appearance of the surface regulation modification layer not only improves the transfer rate of sodium ions, but also improves the surface stability of the material, inhibits side reactions between electrolytes on the surface of the material and the dissolution of transition metal ions, reduces surface cracks, and improves the cyclic stability of the material. Titanium ion doping can improve the environment around the transition metal ions. Since the bond energy of the Ti-O bond is higher than that of the Mn-O and Ni-O bonds, it can enhance the stability of the crystal structure, inhibit the slip of the transition metal layer under high voltage, and at the same time inhibit the lattice distortion and irreversibility of the material, alleviating the effects of Mn 3+ The alkaline substance is used as a sodium source to synthesize the modified layer in situ, which can remove the surface alkalinity and modify the surface at the same time, and play the purpose of isolating the air. It can not only inhibit the side reactions of the battery, but also prevent the cracking of the layered structure and the dissolution of transition metal ions, and improve the electrochemical performance and air stability of the positive electrode material.
[0020] 2. The preparation process of the positive active material of the sodium ion battery of the present invention adjusts the raw material ratio, ultrasonic and microwave process parameters and two-stage heat treatment to adjust the crystal structure, modification layer thickness and material uniformity of the material. Compared with the traditional direct grinding and calcination, the ultrasonic treatment in the solution of the present invention is supplemented by microwave heating to make the raw materials quickly and evenly mixed, the surface modification layer formed is more uniform, the titanium ion doping is uniform, the crystal structure of the material is finely controlled, and the performance and stability of the battery are improved; the two-stage gradient heat treatment first low-temperature heat treatment can orderly control the crystal growth, and then high-temperature treatment further improves the crystal structure, so that the crystal structure of the material is more orderly and stable, and the performance and cycle life of the battery are improved. DETAILED DESCRIPTION
[0021] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0022] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.
[0023] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0024] The ethylene glycol of the present invention exists in the form of a solution, wherein the concentration of the ethylene glycol in the solution is greater than 99.5%.
[0025] The NaNi prepared by the high temperature solid phase method of the present invention 0.5 Mn 0.5 The specific steps are as follows: weigh NaCO3, MnO2, and Ni(OH)2 according to the stoichiometric ratio of n(Na):n(Mn):n(Ni)=2:1:1, grind and mix the materials evenly, put them into a tubular furnace, heat them to 850°C at a rate of 5°C / min in an air atmosphere and keep them warm for 12 hours. After cooling down from the furnace, grind them quickly and store them in a glove box.
[0026] The NaNi prepared by the coprecipitation method of the present invention 0.5 Mn 0.5 O2 The specific steps are: weigh nickel nitrate and manganese nitrate in a molar ratio of 1:1 and place them in a beaker, add 150 ml of deionized water and stir for 2 hours, then slowly pour sodium carbonate aqueous solution (the molar ratio of sodium ion to nickel ion and manganese ion is 2:1:1) into the above metal ion solution, continue stirring for 3 hours, then centrifuge and freeze-dry to obtain a carbonate precipitate, finally, mix and grind the sodium carbonate and carbonate precipitate according to a stoichiometric ratio of 0.03:1, put the evenly mixed material into a tubular furnace, heat to 850°C at a rate of 5°C / min in an air atmosphere and keep warm for 12 hours, quickly grind after cooling with the furnace and store in a glove box.
[0027] The NaNi prepared by the sol-gel method of the present invention 0.5 Mn 0.5 The specific steps of O2 are: weigh sodium acetate, nickel acetate and manganese acetate according to the measurement ratio of n(Na):n(Mn):n(Ni)=2:1:1 and place them in a beaker, add deionized water and stir to dissolve, then add citric acid aqueous solution (the molar ratio of citric acid to metal ions is 3:1) and stir in a water bath for 6 hours to form a gel, dry and grind it and place it in a tubular furnace and heat it to 850°C at a rate of 5°C / min and keep it warm for 12 hours, cool it down in the furnace and grind it quickly and store it in a glove box.
[0028] Example 1
[0029] A method for preparing a positive electrode active material for a sodium ion battery, the specific steps comprising:
[0030] (1) Sodium carbonate, titanium sulfate, sodium phosphate, diammonium phosphate and NaNi in a molar ratio of 1:2.2:3:4:1.04 0.5 Mn 0.5 O2 (prepared by high temperature solid phase method) is added to ethylene glycol, ethylene glycol reacts with NaNi 0.5 Mn 0.5The liquid-to-solid ratio of O2 was 55:1 mL / g, and the solution was ultrasonically stirred at a speed of 350 rpm, a power of 250 W, and a temperature of 35°C for 2 h, and then microwave heated at 450 W and 45°C for 45 min, washed, filtered, and dried to obtain a mixture;
[0031] (2) The mixture was heated to 350°C at a heating rate of 3°C / min for 5 h under a nitrogen atmosphere, and then heated to 700°C at a heating rate of 1°C / min for 6 h to obtain the target sodium ion battery positive electrode active material.
[0032] Example 2
[0033] A method for preparing a positive electrode active material for a sodium ion battery, the specific steps comprising:
[0034] (1) Sodium carbonate, titanium sulfate, sodium phosphate, diammonium phosphate and NaNi in a molar ratio of 1:2.1:3:4:1.03 0.5 Mn 0.5 O2 (prepared by coprecipitation) is added to ethylene glycol, and ethylene glycol reacts with NaNi 0.5 Mn 0.5 The liquid-to-solid ratio of O2 was 50:1 mL / g, and the solution was ultrasonically stirred at a speed of 300 rpm, a power of 200 W, and a temperature of 30°C for 1.5 h, and then microwave heated at 400 W and 40°C for 30 min, washed, filtered, and dried to obtain a mixture;
[0035] (2) The mixture was heated to 300°C at a heating rate of 3°C / min for 4.5 h under a nitrogen atmosphere, and then heated to 650°C at a heating rate of 1°C / min for 5.5 h to obtain the target sodium ion battery positive electrode active material.
[0036] Example 3
[0037] A method for preparing a positive electrode active material for a sodium ion battery, the specific steps comprising:
[0038] (1) Sodium carbonate, titanium sulfate, sodium phosphate, diammonium phosphate and NaNi in a molar ratio of 1:2.3:3:4:1.05 0.5 Mn 0.5 O2 (prepared by sol-gel method) is added to ethylene glycol, and ethylene glycol reacts with NaNi 0.5 Mn 0.5 The liquid-to-solid ratio of O2 was 60:1 mL / g, and the solution was ultrasonically stirred at a speed of 400 rpm, a power of 300 W, and a temperature of 40°C for 2.5 h, and then microwave heated at 500 W and 50°C for 60 min, washed, filtered, and dried to obtain a mixture;
[0039] (2) The mixture was heated to 400°C at a heating rate of 3°C / min for 5.5 h under a nitrogen atmosphere, and then heated to 750°C at a heating rate of 1°C / min for 6.5 h to obtain the target sodium ion battery positive electrode active material.
[0040] Comparative Example 1
[0041] The difference from Example 1 is that the raw materials are sodium carbonate, nickel oxide, manganese dioxide and titanium dioxide in a molar ratio of 2:1:1:0.2, that is, no surface modification is performed, and only titanium ion doping is performed. The rest is the same as Example 1.
[0042] The preparation method of the positive electrode active material of the sodium ion battery in this comparative example comprises the following specific steps:
[0043] (1) Sodium carbonate, nickel oxide, manganese dioxide and titanium dioxide in a molar ratio of 2:1:1:0.2 were added to ethylene glycol, and the liquid-to-solid ratio of ethylene glycol to sodium carbonate was 55:1 mL / g. The solution was ultrasonically stirred at a speed of 350 rpm, a power of 250 W and a temperature of 35°C for 2 h, and then microwaved at 450 W and 45°C for 45 min, washed, filtered and dried to obtain a mixture;
[0044] (2) The mixture was heated to 350°C at a heating rate of 3°C / min for 5 h under a nitrogen atmosphere, and then heated to 700°C at a heating rate of 1°C / min for 6 h to obtain the target sodium ion battery positive electrode active material.
[0045] Comparative Example 2
[0046] The difference from Example 1 is that the molar ratio of sodium carbonate, titanium sulfate, sodium phosphate, ammonium dihydrogen phosphate and NaNi is 1:2:3:4:1.04. 0.5 Mn 0.5 O2, that is, no titanium ion doping, only surface modification. Others are consistent with Example 1.
[0047] The preparation method of the positive electrode active material of the sodium ion battery in this comparative example comprises the following specific steps:
[0048] (1) Sodium carbonate, titanium sulfate, sodium phosphate, diammonium phosphate and NaNi in a molar ratio of 1:2:3:4:1.04 0.5 Mn 0.5 O2 (prepared by high temperature solid phase method) is added to ethylene glycol, ethylene glycol reacts with NaNi 0.5 Mn 0.5The liquid-to-solid ratio of O2 was 55:1 mL / g, and the solution was ultrasonically stirred at a speed of 350 rpm, a power of 250 W, and a temperature of 35°C for 2 h, and then microwave heated at 450 W and 45°C for 45 min, washed, filtered, and dried to obtain a mixture;
[0049] (2) The mixture was heated to 350°C at a heating rate of 3°C / min for 5 h under a nitrogen atmosphere, and then heated to 700°C at a heating rate of 1°C / min for 6 h to obtain the target sodium ion battery positive electrode active material.
[0050] Comparative Example 3
[0051] The difference from Example 1 is that the raw materials are sodium carbonate, titanium dioxide and NaNi in a molar ratio of 1:0.2:1.04. 0.5 Mn 0.5 O2, that is, the surface is modified with sodium carbonate and doped with titanium ions. Others are the same as in Example 1.
[0052] The preparation method of the positive electrode active material of the sodium ion battery in this comparative example comprises the following specific steps:
[0053] (1) Sodium carbonate, titanium dioxide and NaNi in a molar ratio of 1:0.2:1.04 0.5 Mn 0.5 O2 (prepared by high temperature solid phase method) is added to ethylene glycol, ethylene glycol reacts with NaNi 0.5 Mn 0.5 The liquid-to-solid ratio of O2 was 55:1 mL / g, and the solution was ultrasonically stirred at a speed of 350 rpm, a power of 250 W, and a temperature of 35°C for 2 h, and then microwave heated at 450 W and 45°C for 45 min, washed, filtered, and dried to obtain a mixture;
[0054] (2) The mixture was heated to 350°C at a heating rate of 3°C / min for 5 h under a nitrogen atmosphere, and then heated to 700°C at a heating rate of 1°C / min for 6 h to obtain the target sodium ion battery positive electrode active material.
[0055] Comparative Example 4
[0056] The difference from Example 1 is that the raw materials are sodium carbonate, nickel oxide, manganese dioxide and zinc oxide in a molar ratio of 2:1:1:0.2, that is, zinc ion doping. The rest is the same as Example 1.
[0057] The preparation method of the positive electrode active material of the sodium ion battery in this comparative example comprises the following specific steps:
[0058] (1) Sodium carbonate, nickel oxide, manganese dioxide and zinc oxide in a molar ratio of 2:1:1:0.2 were added to ethylene glycol, and the liquid-to-solid ratio of ethylene glycol to sodium carbonate was 55:1 mL / g. The solution was ultrasonically stirred at a speed of 350 rpm, a power of 250 W and a temperature of 35°C for 2 h, and then microwaved at 450 W and 45°C for 45 min, washed, filtered and dried to obtain a mixture;
[0059] (2) The mixture was heated to 350°C at a heating rate of 3°C / min for 5 h under a nitrogen atmosphere, and then heated to 700°C at a heating rate of 1°C / min for 6 h to obtain the target sodium ion battery positive electrode active material.
[0060] Comparative Example 5
[0061] The difference from Example 1 is that the preparation method is grinding + high-temperature calcination. The rest is the same as Example 1.
[0062] The preparation method of the positive electrode active material of the sodium ion battery in this comparative example comprises the following specific steps:
[0063] (1) Sodium carbonate, titanium sulfate, sodium phosphate, diammonium phosphate and NaNi in a molar ratio of 1:2.2:3:4:1.04 0.5 Mn 0.5 O2 is ground and mixed uniformly to obtain a mixture;
[0064] (2) The mixture was heated to 700°C at a heating rate of 3°C / min under a nitrogen atmosphere and sintered for 6 h to obtain the target sodium ion battery positive electrode active material.
[0065] Comparative Example 6
[0066] The difference from Example 1 is that the preparation method lacks microwave heating. Other aspects are the same as Example 1.
[0067] The preparation method of the positive electrode active material of the sodium ion battery in this comparative example comprises the following specific steps:
[0068] (1) Sodium carbonate, titanium sulfate, sodium phosphate, diammonium phosphate and NaNi in a molar ratio of 1:2.2:3:4:1.04 0.5 Mn 0.5 O2 (prepared by high temperature solid phase method) is added to ethylene glycol, ethylene glycol reacts with NaNi 0.5 Mn 0.5 The liquid-to-solid ratio of O2 was 55:1 mL / g, and the solution was ultrasonically stirred for 2 h at a speed of 350 rpm, a power of 250 W, and a temperature of 35°C, washed, filtered, and dried to obtain a mixture;
[0069] (2) The mixture was heated to 350°C at a heating rate of 3°C / min for 5 h under a nitrogen atmosphere, and then heated to 700°C at a heating rate of 1°C / min for 6 h to obtain the target sodium ion battery positive electrode active material.
[0070] Application Examples
[0071] Preparation of sodium ion battery: The sodium ion battery positive electrode active material, Ketjen black, and PVDF (polyvinylidene fluoride) binder prepared in Examples 1-3 and Comparative Examples 1-6 were weighed in a mass ratio of 8:1:1 and mixed evenly, and an appropriate amount of N-methyl-2-pyrrolidone solvent was added to form a slurry, which was evenly coated on aluminum foil using a scraper, dried in a vacuum drying oven for 12 hours, and made into a positive electrode sheet (12 mm disc). In a glove box filled with argon (H2O, O2 <0.01ppm), the positive electrode sheet, metal sodium sheet, glass fiber separator, electrolyte NaClO4 / PC (sodium perchlorate / propylene carbonate), and nickel foam were assembled into button cells in sequence, and the assembled button cells were left to stand for 12 hours for testing.
[0072] The test results are shown in Table 1-2.
[0073] Table 1
[0074]
[0075] Table 2
[0076]
[0077] It can be seen from Table 1 that the sodium ion batteries assembled with the sodium ion battery positive electrode active materials prepared in Examples 1-3 of the present invention have good electrochemical performance, and the first discharge specific capacity and coulombic efficiency are better than those of Comparative Examples 1-6.
[0078] As can be seen from Table 2, the sodium ion battery assembled with the sodium ion battery positive electrode active material prepared in Examples 1-3 of the present invention has good cycle performance, and the capacity retention rate after 100 cycles of charge and discharge is not less than 90% at 0.1C and not less than 80% at 5C, while the capacity retention rate of Comparative Examples 1-5 after 100 cycles of charge and discharge is reduced to varying degrees. In addition, the sodium ion battery prepared in Examples 1-3 has good stability, and the material capacity retention rate is not less than 85% after 60 days of air storage, while the stability performance of Comparative Examples 1-6 is reduced.
[0079] It can be concluded from Table 1-2 that the present invention uses surface regulation and modification and ion doping to treat layered oxides (NaNi 0.5 Mn 0.5 O2) materials are synergistically modified, and the two work together to improve the electrochemical performance and air stability of the positive electrode materials.
[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a positive electrode active material for a sodium ion battery, characterized in that: The specific steps include: (1) Sodium carbonate, titanium sulfate, phosphate and NaNi 0.5 Mn 0.5 O2 is added to ethylene glycol, ultrasonically stirred, assisted by microwave heating, washed, filtered, and dried to obtain a mixture; The ultrasonic stirring time is 1.5-2.5h, the speed is 300-400rpm, the power is 200-300W, and the temperature is 30-40°C; The microwave heating is carried out at 400-500W and 40-50°C for 30-60min; The sodium carbonate, titanium sulfate, phosphate and NaNi 0.5 Mn 0.5 The molar ratio of O2 is 1:(2.1-2.3):7:(1.03-1.05); The phosphate is composed of sodium phosphate and ammonium dihydrogen phosphate in a molar ratio of 3:4; (2) The mixture is heat treated twice in a nitrogen inert atmosphere, firstly the temperature is increased to 300-400°C at a heating rate of 3°C / min for 4.5-5.5h, and then the temperature is increased to 650-750°C at a heating rate of 1°C / min for 5.5-6.5h to obtain the target sodium ion battery positive electrode active material.
2. The method for preparing a positive electrode active material for a sodium ion battery according to claim 1, characterized in that: In step (1), the NaNi 0.5 Mn 0.5 O2 is prepared by high temperature solid phase method, coprecipitation method or sol-gel method.
3. The method for preparing a positive electrode active material for a sodium ion battery according to claim 1, characterized in that: In step (1), the ethylene glycol and NaNi 0.5 Mn 0.5 The liquid-to-solid ratio of O2 is 50-60:1mL / g.
4. A positive electrode active material for a sodium ion battery, characterized in that: The method is prepared according to any one of claims 1 to 3.