A kind of silt solidifying agent based on mineral powder, preparation method and application thereof
Through the combination of ore powder, calcium hydroxide, sodium sulfate and modified composite fiber, the strength of silt is improved by using the gelling and filling effects, the problems of brittleness and environmental pollution of ore powder curing agent are solved, and high-performance silt curing is achieved The preparation of agents meets the sustainable development needs of construction projects.
Patent Information
- Application Number
- CN202410731135.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-06-06
AI Technical Summary
As a silt curing agent, existing ore powder has problems such as high brittleness and insufficient toughness, which is difficult to meet the high performance requirements of new materials in construction projects. The cement production process is highly polluted to the environment, and requires a sustainable resource utilization. method.
Using the combination of ore powder, calcium hydroxide, sodium sulfate and modified composite fiber powder, the strength of the silt is improved through the gelation effect and filling effect, the hydration reaction of ore powder is used to generate gel substances, and through carbon fiber and glass fiber The composite material enhances the connection strength of the gelled substance.
The silt soil has significantly improved the 7d unbounded compressive strength, 7d splitting strength and water stability coefficient, forming a high-performance composite material, meeting the sustainable development needs of construction projects, saving resources and reducing environmental pollution.
Smart Images

Figure CN118619634B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of industrial solid waste utilization, and in particular to a silt solidifying agent based on mineral powder, a preparation method and application thereof. Background Art
[0002] Silt is widely distributed in the alluvial plains of the middle and lower reaches of the Yellow River in my country. It has poor gradation, weak cohesion, and low strength, which makes it difficult to meet the performance requirements of roadbed fillers. In order to improve the bearing capacity of silt roadbed, it is usually stabilized by improving the curing agent in engineering. Soil curing agents can generally undergo a series of physical and chemical reactions with soil at room temperature to generate gelling substances, effectively improving the mechanical properties and durability of the soil.
[0003] The most common solidifying material at present is cement, and many scholars will use it in combination with some industrial waste. The combination of cement and industrial waste will stimulate the active substances in the soil to react with volcanic ash to produce cementitious substances. These products overlap each other and fill the voids in the soil, connecting the soil particles into a whole, thereby increasing the strength of the soil and maintaining the performance basically unchanged for a long time. However, in the process of producing cement, a large amount of natural resources such as natural clay and fossil energy will be consumed, and a large amount of harmful gases will be discharged, thereby polluting the environment and not in line with the country's green and sustainable development strategy.
[0004] With the gradual acceleration of my country's industrialization process, a large amount of industrial solid waste is generated every year. Industrial solid waste refers to various waste slag, dust and other wastes generated in industrial production activities. It can be subdivided into general industrial wastes and industrial hazardous solid wastes such as blast furnace slag, steel slag, red mud, fly ash, waste gypsum, and calcium carbide slag. Not only is it very troublesome to classify and treat, but the storage method occupies a large amount of land resources and is very likely to cause ecological damage. Therefore, how to utilize it as a resource has a strong reality and urgency. Slag, as an industrial waste generated in the process of smelting pig iron, mainly contains calcium, silicon, aluminum, sulfide and a small amount of iron and magnesium oxides. It has high potential activity. When added to the soil, it will cement and compact the soil particles to achieve the effect of improved solidification. And it has many advantages such as low price, easy transportation and storage, energy saving and environmental protection. Despite this, the mineral powder prepared with slag as the basic raw material of the silt curing agent still has the problem of large brittleness and insufficient toughness, which cannot meet people's sustainable and high-performance requirements for the use of new materials, limiting its application in construction engineering materials.
[0005] Therefore, the preparation of a silt reinforcement agent that has high strength and can utilize industrial solid waste such as slag is of great significance for the future development of road engineering and other construction fields. Summary of the invention
[0006] The object of the present invention is to provide a silt solidifying agent based on mineral powder, a preparation method and application thereof, so as to solve the problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A powdered soil curing agent based on mineral powder, comprising the following components by weight: 60-75 parts of mineral powder, 26-39 parts of calcium hydroxide, 2-4 parts of sodium sulfate and 3-4 parts of modified composite fiber powder, wherein the mineral powder is ground to a specific surface area of 400-500m 2 / kg of fine powder.
[0009] Preferably, the method for preparing the modified composite fiber comprises the following steps:
[0010] S101: dispersing glass fibers in ethanol, adding aminopropyl dimethoxysilane to the ethanol, treating the glass fibers in the ethanol solution containing aminopropyl dimethoxysilane for 2-3 hours, and emitting ultrasonic waves into the ethanol solution while the glass fibers are immersed;
[0011] S102: placing the carbon fiber in a concentrated nitric acid solution for 0.8-2 hours and heating it to 65° C., and washing the product after the concentrated nitric acid is filtered with ethanol;
[0012] S103: putting the carbon fiber washed with ethanol in step S102 into the ethanol solution containing glass fiber in step S101, adding bisphenol A epoxy resin, stirring at 50-60° C. for 1-2.5 hours, filtering, and drying to obtain modified composite fiber;
[0013] S104: mechanically grinding the modified composite fiber obtained in step S103 into powder, and heating it at 130-150° C. during the grinding process to obtain modified composite fiber powder.
[0014] Preferably, in step S101, the mass ratio of aminopropyldimethoxysilane to ethanol is (2-4):50, and the frequency of the ultrasonic wave is 22.3-25.8 KHz.
[0015] Preferably, the molar concentration of the concentrated nitric acid solution in step S102 is 14.2-16.5.
[0016] Preferably, the mass ratio of the bisphenol A epoxy resin, carbon fiber and glass fiber is 1:(3-7):(8-24).
[0017] A method for preparing the above-mentioned mineral powder-based silt solidifying agent comprises the following steps:
[0018] S1: Dry the mineral powder, calcium hydroxide and sodium sulfate in an oven, then grind and sieve them thoroughly. The grinding time is 40-60 minutes.
[0019] S2: putting the powder obtained in step S1 into a mixer, adding the modified composite fiber powder into the mixer, controlling the speed of the mixer to 200-300 r / min, and stirring for 10-20 min;
[0020] S3: placing the powder mixed in step S2 in a sealed bag and storing it at room temperature to form a powder curing agent based on mineral powder.
[0021] The invention discloses an application of a mineral powder-based silt solidifying agent in solidifying roadbed soil in road engineering.
[0022] Preferably, the application of the mineral powder-based soil solidifying agent in roadbed soil solidification of road engineering adopts the following method:
[0023] The finished powder curing agent based on mineral powder is added to the roadbed soil of the road project at a dosage of 12%, and then prepared into a cured soil mixture at an optimal moisture content of 11.2%, and cured for 7 days in an environment of 18-22°C and a relative humidity greater than 95%.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The silt solidifying agent based on mineral powder and solid waste provided by the present invention mainly achieves the purpose of silt improvement through gelling effect and filling effect. When the mineral powder is ground into mineral powder and placed in an alkaline environment, the activity of the silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron therein is stimulated, and the reaction generates gel substances such as hydrated calcium silicate and hydrated calcium aluminate. As the hydration reaction continues, the gel substances are continuously connected and polymerized, filling the pores of the soil and overlapping the soil particles, thereby increasing the contact area of the soil particles, so that the dispersed soil particles form an overall spatial network. The present invention uses mineral powder as a silt solidifying agent, fully utilizes the mineral powder as solid waste, and saves resources;
[0026] 2. In the present invention, a composite material of carbon fiber and glass fiber is added to the curing agent based on mineral powder. In the process of continuous connection, polymerization and filling of soil pores by the gelling material, it is jointly wrapped by the gelling material and overlapped with the soil particles to form a composite material with higher connection strength. The composite material is attached to the surface of the soil, which greatly improves the strength of the silt when the curing agent acts on the silt. In addition, the compounding of carbon fiber and glass fiber also reduces the cost of using carbon fiber alone. The 7d unconfined compressive strength, 7d splitting strength and water stability coefficient of the mineral powder composite cured soil are improved compared with the cement cured soil in the comparative example. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1The process flow chart of the preparation method of the silt solidifying agent based on mineral powder in the present invention;
[0028] Figure 2 is a process flow chart of the modified fiber preparation method of the present invention;
[0029] Figure 3 This is a schematic diagram of a silt solidifying agent product based on mineral powder prepared by the present invention;
[0030] Figure 4 is the X-ray diffraction spectrum of the road engineering subgrade soil used in the present invention;
[0031] Figure 5 The X-ray diffraction spectrum of roadbed soil of a road project after adding the mineral powder-based silt curing agent prepared in Example 1 of the present invention;
[0032] Figure 6 This is a SEM image of the roadbed soil used in the present invention;
[0033] Figure 7 This is a SEM image of roadbed soil in a road engineering project after adding the mineral powder-based silt solidifier prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The mineral powder used in the present invention is selected from the S95 grade slag powder produced by Gongyi Longze Water Purification Material Co., Ltd., which has an off-white appearance, a 7d activity index of 84.2%, a 28d activity index of 98.5%, a density of 3.1g / cm3, a loss on ignition of 0.84%, and a water content of 0.5%. Its main components are CaO, SiO2, and Al2O3, accounting for about 86% of the total amount, and also contains a small amount of MgO, Fe2O3, etc. The mineral powder is ground to a specific surface area of 400-500m 2 / kg fine powder, the basic chemical composition is shown in Table 1:
[0036] Table 1: Basic chemical composition of mineral powder used in the present invention
[0037]
[0038] The calcium hydroxide used in the present invention is selected from Tianjin Zhiyuan Chemical Reagent Co., Ltd. and is a white crystalline powder with a purity of ≥95%. The specific chemical composition is shown in Table 2 below:
[0039] Table 2: Basic chemical composition of calcium hydroxide used in the present invention
[0040]
[0041] Table 3: Basic chemical composition of sodium sulfate used in the present invention
[0042]
[0043] The roadbed soil used in the present invention is taken from the underground depth of 150 cm at the site of the Henan Anhe Expressway Project. It is a low liquid limit silt with high powder content, poor gradation, low plasticity index, low shear strength, and strong capillary action. It cannot meet the requirements of highway roadbed fillers. Its basic physical property indicators and particle size distribution are shown in Tables 4 and 5 below:
[0044] Table 4: Basic physical property indexes of road engineering subgrade soil used in the present invention
[0045]
[0046] Table 5: Particle size distribution of roadbed soil particles used in the present invention
[0047] Aperture / mm 5 2 1 0.5 0.25 0.075 Pass rate / % 100 86.5 78.4 70.3 66.7 60.2
[0048] See also Figure 1-Figure 7 , the present invention provides a technical solution:
[0049] Example 1
[0050] A method for preparing a silt solidifying agent based on mineral powder, comprising the following steps:
[0051] S1: 63g of specific surface area of 450m 2 / kg of mineral powder, 34g of calcium hydroxide and 3g of sodium sulfate are dried in an oven, then fully ground and sieved, and the grinding time is 40min;
[0052] S2: putting the powder obtained in step S1 into a mixer, adding 3 g of modified composite fiber powder into the mixer, controlling the speed of the mixer to 200 r / min, and stirring for 10 min;
[0053] S3: placing the powder mixed in step S2 in a sealed bag and storing it at room temperature to form a powder curing agent based on mineral powder.
[0054] The modified composite fiber powder in step S2 is prepared by the following steps:
[0055] S101: 8 g of glass fiber is dispersed in 50 g of ethanol, 2 g of aminopropyl dimethoxysilane is added to the ethanol, and the glass fiber is treated in the ethanol solution containing aminopropyl dimethoxysilane for 3 hours. While the glass fiber is immersed, 25.8 KHz ultrasonic waves are simultaneously emitted into the ethanol solution;
[0056] S102: 3 g of carbon fiber is placed in 50 ml of concentrated nitric acid solution for 2 h and heated to 65° C. The product after the concentrated nitric acid is filtered is washed with ethanol. The molar concentration of the concentrated nitric acid solution is 14.2.
[0057] S103: putting the carbon fiber washed with ethanol in step S102 into the ethanol solution containing glass fiber in step S101, adding 1 g of bisphenol A epoxy resin, stirring at 60° C. for 2.5 h, filtering, and drying to obtain modified composite fiber;
[0058] S104: mechanically grinding the modified composite fiber obtained in step S103 into powder, and heating it at 130° C. during the grinding process to obtain modified composite fiber powder.
[0059] Example 2
[0060] A method for preparing a silt solidifying agent based on mineral powder, comprising the following steps:
[0061] S1: 67g of specific surface area of 400m 2 / kg of mineral powder, 30g of calcium hydroxide and 3g of sodium sulfate are dried in an oven, then fully ground and sieved, and the grinding time is 60min;
[0062] S2: putting the powder obtained in step S1 into a mixer, adding 4 g of modified composite fiber powder into the mixer, controlling the speed of the mixer to 300 r / min, and stirring for 20 min;
[0063] S3: placing the powder mixed in step S2 in a sealed bag and storing it at room temperature to form a powder curing agent based on mineral powder.
[0064] The modified composite fiber powder in step S2 is prepared by the following steps:
[0065] S101: 24 g of glass fiber is dispersed in 200 g of ethanol, 16 g of aminopropyl dimethoxysilane is added to the ethanol, and the glass fiber is treated in the ethanol solution containing aminopropyl dimethoxysilane for 2 hours. While the glass fiber is immersed, 25.8 KHz ultrasonic waves are simultaneously emitted into the ethanol solution;
[0066] S102: 7 g of carbon fiber is placed in 80 ml of concentrated nitric acid solution for treatment for 0.8 h, and heated to 65° C., and the product after the concentrated nitric acid is filtered is washed with ethanol, and the molar concentration of the concentrated nitric acid solution is 16.5;
[0067] S103: putting the carbon fiber washed with ethanol in step S102 into the ethanol solution containing glass fiber in step S101, adding 1 g of bisphenol A epoxy resin, stirring at 60° C. for 1 h, filtering, and drying to obtain modified composite fiber;
[0068] S104: mechanically grinding the modified composite fiber obtained in step S103 into powder, and heating it at 150° C. during the grinding process to obtain modified composite fiber powder.
[0069] Example 3
[0070] A method for preparing a silt solidifying agent based on mineral powder, comprising the following steps:
[0071] S1: 60g of specific surface area of 400m 2 / kg of mineral powder, 37g of calcium hydroxide and 3g of sodium sulfate were dried in an oven, then fully ground and sieved, and the grinding time was 45min;
[0072] S2: Put the powder obtained in step S1 into a mixer, add 3g of modified composite fiber powder into the mixer, control the mixer speed to 240r / min, and stir for 15min;
[0073] S3: placing the powder mixed in step S2 in a sealed bag and storing it at room temperature to form a powder curing agent based on mineral powder.
[0074] The modified composite fiber powder in step S2 is prepared by the following steps:
[0075] S101: 17 g of glass fiber is dispersed in 150 g of ethanol, 9 g of aminopropyl dimethoxysilane is added to the ethanol, and the glass fiber is treated in the ethanol solution containing aminopropyl dimethoxysilane for 2.8 h. While the glass fiber is immersed, 24.2 kHz ultrasonic waves are simultaneously emitted into the ethanol solution;
[0076] S102: 5 g of carbon fiber is placed in 60 ml of concentrated nitric acid solution for 1.1 h and heated to 65° C. The product after the concentrated nitric acid is filtered is washed with ethanol. The molar concentration of the concentrated nitric acid solution is 15.8;
[0077] S103: putting the carbon fiber washed with ethanol in step S102 into the ethanol solution containing glass fiber in step S101, adding 1 g of bisphenol A epoxy resin, stirring at 55° C. for 1.9 h, filtering, and drying to obtain modified composite fiber;
[0078] S104: mechanically grinding the modified composite fiber obtained in step S103 into powder, and heating it at 140° C. during the grinding process to obtain modified composite fiber powder.
[0079] Example 4
[0080] A method for preparing a silt solidifying agent based on mineral powder, comprising the following steps:
[0081] S1: 72g specific surface area 430m 2 / kg of mineral powder, 26g of calcium hydroxide and 2g of sodium sulfate are dried in an oven, then fully ground and sieved, and the grinding time is 50min;
[0082] S2: Put the powder obtained in step S1 into a mixer, add 3g of modified composite fiber powder into the mixer, control the mixer speed to 240r / min, and stir for 15min;
[0083] S3: placing the powder mixed in step S2 in a sealed bag and storing it at room temperature to form a powder curing agent based on mineral powder.
[0084] The modified composite fiber powder in step S2 is prepared by the following steps:
[0085] S101: 17 g of glass fiber is dispersed in 150 g of ethanol, 9 g of aminopropyl dimethoxysilane is added to the ethanol, and the glass fiber is treated in the ethanol solution containing aminopropyl dimethoxysilane for 2.8 h. While the glass fiber is immersed, 24.2 kHz ultrasonic waves are simultaneously emitted into the ethanol solution;
[0086] S102: 5 g of carbon fiber is placed in 60 ml of concentrated nitric acid solution for 1.1 h, and the product after the concentrated nitric acid is filtered is washed with ethanol, and the molar concentration of the concentrated nitric acid solution is 15.8;
[0087] S103: putting the carbon fiber washed with ethanol in step S102 into the ethanol solution containing glass fiber in step S101, adding 1g of bisphenol A type epoxy resin, stirring at 55° C. for 1.9 hours, filtering, and drying to obtain modified composite fiber;
[0088] S104: mechanically grinding the modified composite fiber obtained in step S103 into powder, and heating it at 140° C. during the grinding process to obtain modified composite fiber powder.
[0089] Example 5
[0090] A method for preparing a silt solidifying agent based on mineral powder, comprising the following steps:
[0091] S1: 57g specific surface area is 480m 2 / kg of mineral powder, 39g of calcium hydroxide and 4g of sodium sulfate were dried in an oven, then fully ground and sieved, and the grinding time was 50min;
[0092] S2: putting the powder obtained in step S1 into a mixer, adding 4 g of modified composite fiber powder into the mixer, controlling the speed of the mixer to 200 r / min, and stirring for 10 min;
[0093] S3: placing the powder mixed in step S2 in a sealed bag and storing it at room temperature to form a powder curing agent based on mineral powder.
[0094] The modified composite fiber powder in step S2 is prepared by the following steps:
[0095] S101: 17 g of glass fiber is dispersed in 150 g of ethanol, 9 g of aminopropyl dimethoxysilane is added to the ethanol, and the glass fiber is treated in the ethanol solution containing aminopropyl dimethoxysilane for 2.8 h. While the glass fiber is immersed, 24.2 kHz ultrasonic waves are simultaneously emitted into the ethanol solution;
[0096] S102: 5 g of carbon fiber is placed in 60 ml of concentrated nitric acid solution for 1.1 h, and the product after the concentrated nitric acid is filtered is washed with ethanol, and the molar concentration of the concentrated nitric acid solution is 15.8;
[0097] S103: putting the carbon fiber washed with ethanol in step S102 into the ethanol solution containing glass fiber in step S101, adding 1 g of bisphenol A epoxy resin, stirring at 55° C. for 1.9 h, and drying to obtain modified composite fiber;
[0098] S104: mechanically grinding the modified composite fiber obtained in step S103 into powder, and heating it at 140° C. during the grinding process to obtain modified composite fiber powder.
[0099] Comparative Example 1
[0100] Compared with Example 1, in Comparative Example 1, ground glass fiber is directly added in step S2, the amount of glass fiber and modified composite fiber powder used is the same, and the remaining steps are exactly the same as in Example 1.
[0101] Comparative Example 2
[0102] Compared with Example 1, in Comparative Example 2, ground carbon fiber is directly added in step S2, the amount of carbon fiber and modified composite fiber powder used is the same, and the remaining steps are exactly the same as in Example 1.
[0103] Comparative Example 3
[0104] Compared with Example 1, in Comparative Example 3, neither glass fiber nor carbon fiber is added in step S2, and the remaining steps are exactly the same as those in Example 1.
[0105] Comparative Example 4
[0106] Compared with Example 1, Comparative Example 4 eliminates the addition of mineral powder, calcium hydroxide and sodium sulfate, and instead adds modified composite fiber powder to the ordinary Portland cement of Conch brand PO42.5.
[0107] Comparative Example 5
[0108] Comparative Example 4 Compared with Example 1, the addition of mineral powder, calcium hydroxide, sodium sulfate and modified composite fiber powder was omitted, and ordinary Portland cement of Conch brand PO 42.5 was directly used as a control experiment.
[0109] The reinforcing agent powder prepared in the above 10 implementation methods and the ordinary Portland cement of Conch brand PO 42.5 were added to the roadbed soil of the road engineering at an amount of 12%, and then a solidified soil mixture was prepared at an optimal moisture content of 11.2%. After being mixed evenly, a cylindrical sample with a diameter × height = 50 mm × 50 mm was prepared by static compaction method according to the "Testing Procedure for Stabilized Materials of Inorganic Binders for Highway Engineering" (JTG E51-2009), and was placed in a standard curing room with a temperature of 20°C ± 2°C and a relative humidity greater than 95% for curing for 7 days. After the curing was completed, the 7d unconfined compressive strength, 7d splitting strength and water stability coefficient of the solidified soil were measured. The measurement results are shown in Table 6 below:
[0110] Table 6: Experimental data table of various implementation methods
[0111]
[0112] It can be seen from Table 6 that the 7d unconfined compressive strength, 7d splitting strength and water stability coefficient of the mineral powder composite solidified soil in the embodiment of the present invention are improved compared with the cement solidified soil in the comparative example. According to the test data in Table 6, the optimal mix ratio of the mineral powder-based silt solidifying agent provided by the present invention is mineral powder: calcium hydroxide: sodium sulfate: modified composite fiber powder = 63:34:3:3. When it is applied to silt, the solidified soil has a 7d unconfined compressive strength of 4.33 MPa, a 7d splitting strength of 0.58 MPa, and a water stability coefficient of 65.8%.
[0113] In the present invention, the strength of silt is improved through the gelling effect and filling effect of the mineral powder itself. The filling effect refers to the fact that the fine mineral powder particles and the mineral powder hydration gelling products jointly fill the gaps between the soil particles, thereby improving the density of the soil and forming a dense whole. The gelling effect can be mainly divided into the self-hydration, excitation, ion exchange and carbonation of the curing agent. The self-hydration of the mineral powder refers to the fact that the blast furnace slag particles are larger after quenching in water and do not undergo any chemical reaction in water. At the same time, combined with composite fibers, the strength of the formed gelling material is further enhanced, providing a new idea for the efficient utilization of mineral powder.
[0114] pass Figure 4 and Figure 5 It can be seen that after using the silt solidifying agent prepared in Example 1 of the present invention, it is beneficial to the formation of calcium silicate hydrate and accelerate the solidification of the roadbed soil. Figure 6 and Figure 7 It can be seen that after using the silt solidifying agent prepared in Example 1 of the present application, the degree of fiberization is obvious, so that the silt solidifying agent successfully adheres to the surface of the roadbed soil, successfully acts on the roadbed soil, clusters on the surface of the roadbed soil, and the two are successfully compounded.
[0115] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A silt solidifier based on mineral powder, characterized in that: The composition comprises the following components by weight: 60-75 parts of mineral powder, 26-39 parts of calcium hydroxide, 2-4 parts of sodium sulfate and 3-4 parts of modified composite fiber powder, wherein the mineral powder is ground to a specific surface area of 400-500m 2 / kg of fine powder; The preparation method of the modified composite fiber comprises the following steps: S101: dispersing glass fibers in ethanol, adding aminopropyl dimethoxysilane to the ethanol, treating the glass fibers in the ethanol solution containing aminopropyl dimethoxysilane for 2-3 hours, and emitting ultrasonic waves into the ethanol solution while the glass fibers are immersed; S102: placing the carbon fiber in a concentrated nitric acid solution for 0.8-2 hours and heating it to 65° C., and washing the product after the concentrated nitric acid is filtered with ethanol; S103: putting the carbon fiber washed with ethanol in step S102 into the ethanol solution containing glass fiber in step S101, adding bisphenol A epoxy resin, stirring at 50-60° C. for 1-2.5 hours, filtering, and drying to obtain modified composite fiber; S104: mechanically grinding the modified composite fiber obtained in step S103 into powder, and heating it at 130-150° C. during the grinding process to obtain modified composite fiber powder; In step S101, the mass ratio of aminopropyldimethoxysilane to ethanol is (2-4):50, and the frequency of the ultrasonic wave is 22.3-25.8 KHz; The molar concentration of the concentrated nitric acid solution in step S102 is 14.2-16.5; The mass ratio of the bisphenol A epoxy resin, carbon fiber and glass fiber is 1:(3-7):(8-24).
2. A method for preparing a silt solidifying agent based on mineral powder as claimed in claim 1, characterized in that: The following steps are involved: S1: Dry the mineral powder, calcium hydroxide and sodium sulfate in an oven, then grind and sieve them thoroughly. The grinding time is 40-60 minutes. S2: putting the powder obtained in step S1 into a mixer, adding the modified composite fiber powder into the mixer, controlling the speed of the mixer to 200-300 r / min, and stirring for 10-20 min; S3: placing the powder mixed in step S2 in a sealed bag and storing it at room temperature to form a powder curing agent based on mineral powder.
3. Use of the mineral powder-based silt solidifier according to claim 1 or the mineral powder-based silt solidifier prepared by the preparation method according to claim 2 in solidifying roadbed soil in road engineering.
4. The use of a mineral powder-based soil solidifying agent in roadbed soil solidification of a road engineering project according to claim 3, characterized in that: Use the following method: The finished powder curing agent based on mineral powder is added to the roadbed soil of the road project at a dosage of 12%, and then prepared into a cured soil mixture at an optimal moisture content of 11.2%, and cured for 7 days in an environment of 18-22°C and a relative humidity greater than 95%.