A preparation method of a twin-crystal structure high entropy (Ti, M) (C, N) based cermet

Through the high-energy ball milling and vacuum sintering process of high-entropy alloys and ceramic solid solution powder, the problems of element diffusion and grain dissolution of metal cermets during sintering are solved, and high hardness, high strength, toughness, and high entropy (Ti, M)(C,N)-based cermets realize the improvement of the comprehensive mechanical properties of the materials and industrial applications.

CN118621170BActive Publication Date: 2024-11-19SUZHOU LABORATORY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411111191.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-19
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The prior art is difficult to slow down the diffusion of metal cermet elements and dissolution of grains during the sintering process, making it difficult to prepare high-hardness, high-strength and toughness metal cermets with dual crystal structures and uniform and dense.

Method used

High-entropy alloy and ceramic solid solution powder are used to prepare high-entropy alloy bonding phase and (Ti,M)(C,N) ceramic solid solution powder through high-entropy ball mill. Combined with wet grinding and vacuum sintering technology, a double crystal structure high-entropy (Ti) is formed. ,M)(C,N)-based cermet, reduces the sintering temperature and improves the comprehensive mechanical properties of the material.

Benefits of technology

It has achieved the improvement of the fracture toughness and comprehensive mechanical properties of metal cermet under high hardness conditions, significantly improved hardness and toughness, and the process is simple, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118621170B_ABST
    Figure CN118621170B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a twin-crystal structure high entropy (Ti, M) (C, N)-based cermet, the steps of which are: preparing a high entropy alloy mixture with Fe, Co, Ni, Ti and Mo as raw materials, and preparing a high entropy alloy mixture with TiC, TiN and Mo as raw materials. 2 C.Cr 3 C 2 , VC, and TaC are used as raw materials to prepare a (Ti, M) (C, N) ceramic solid solution powder mixture, which is prepared with a mass percentage of Fe: 1.58~3.91wt%, Co: 1.67~4.13wt%, Ni: 1.66~4.11wt%, Ti: 21.27~22.51wt%, Mo: 18.00~18.24wt%, Cr: 9.37~12.43wt%, V: 3.06~4.06wt%, Ta: 10.86~14.42wt%, O: 8.50~8.65wt%, C: 14.18~15.42wt%, and N: 0.94~1.03wt%. The high-entropy metal ceramic tools prepared by this method have higher hardness and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a twin-crystal structure high-entropy (Ti, M) (C, N)-based cermet, belonging to the technical field of powder metallurgy. Background Art

[0002] With the continuous development of science and technology, the difficult-to-process materials used in aviation, aerospace, automobile and other fields have increased year by year. Especially in the process of manufacturing aerospace parts that pursue high performance and high precision, the cutting of difficult-to-process materials has always been a key issue restricting production efficiency and product quality. How to maintain stable cutting performance in extreme working environments, improve processing efficiency, and ensure the accuracy and reliability of processed parts at the same time, which brings new challenges to the future tooling industry. Ti (C, N)-based cermets have been widely used in many fields at home and abroad due to their own advantages such as high hardness, high wear resistance, high strength and toughness, high red hardness and excellent chemical stability. In order to give cermets excellent comprehensive mechanical properties, that is, to significantly enhance their strength and toughness while maintaining high hardness, a bi-crystalline structure cermet with a hard phase grain size showing a bimodal distribution has become a research hotspot in recent years. Due to the simultaneous existence of coarse and fine grains in the microstructure, it combines the high strength and toughness of coarse-grained cermets and the high hardness of fine-grained cermets, thereby achieving excellent comprehensive mechanical properties. However, due to the dissolution-precipitation mechanism during the sintering process, most fine particles tend to dissolve first, precipitate and grow on the surface of large particles. This natural process makes it extremely difficult to prepare ideal twin-crystal structure metal ceramics by traditional methods. Although the preparation methods of Ti(C,N)-based metal ceramics with mixed crystal structures disclosed in patents CN 109576545 B and CN 113025861 B have improved the comprehensive mechanical properties of metal ceramics to a certain extent, the hardness value of metal ceramics is relatively low. Therefore, it is particularly important to slow down the diffusion of elements and the dissolution of grains in the sintering process of metal ceramics to prepare metal ceramics with twin crystal structures that are uniform and dense.

[0003] The preparation of cermets by mixed sintering of high entropy alloy or high entropy ceramic powders has been another hot topic in the field of cermet research in recent years. This is mainly due to the high entropy effect in thermodynamics, the slow diffusion effect in kinetics, the high stability of the organization, the lattice distortion effect in structure and the "cocktail" effect of performance brought by high entropy powders, which make high entropy cermets have higher hardness and toughness than traditional cermets. If these characteristics of high entropy powders are directly applied to the preparation of twin-crystal structured cermets, the diffusion of alloying elements and the dissolution of fine particles during the sintering process can be well slowed down, so that the preparation of twin-crystal structured cermets can be completed through a simple sintering process.

[0004] Therefore, how to prepare a twin-crystal structure high-entropy metal ceramic with uniform density, high hardness and high toughness through a simple and low-cost process is the main goal of this patent. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a twin-crystal structure high-entropy (Ti, M) (C, N)-based cermet, which adopts high-entropy alloy and ceramic solid solution powder to prepare cermet materials having a twin-crystal structure in addition to the microstructure, so as to solve the problem that the fracture toughness of cermets is low under high hardness conditions and the comprehensive mechanical properties are not high.

[0006] This application is implemented through the following technical solutions:

[0007] The components of the Ti(C,N)-based metal ceramic are as follows: Fe: 1.58-3.91wt%, Co: 1.67-4.13wt%, Ni: 1.66-4.11wt%, Ti: 21.27-22.51wt%, Mo: 18.00-18.24wt%, Cr: 9.37-12.43wt%, V: 3.06-4.06wt%, Ta: 10.86-14.42wt%, O: 8.50-8.65wt%, C: 14.18-15.42wt%, and N: 0.94-1.03wt%.

[0008] Furthermore, in the above-mentioned components, the high entropy alloy binder phase is introduced by Fe, Co, Ni, Ti, and Mo single metal powders, C is introduced by various metal carbide powders and graphite, N is introduced by TiN, and O is introduced by TiO 2 The particle size of the single metal powder is 2-4 μm, the particle size of the metal carbide powder is 3-6 μm, the particle size of the graphite powder is 1-2 μm, and the particle size of the TiO 2 The particle size of the powder is 0.2 to 0.5 μm.

[0009] The present invention also provides a method for preparing a twin-crystal structure high-entropy (Ti, M) (C, N)-based cermet, comprising the following steps:

[0010] (1) Preparation of high entropy alloy mixture: Fe, Co, Ni, Ti, and Mo are used as raw materials to prepare a mixture with a mass percentage of: Fe: 1.58-3.91wt%, Co: 1.67-4.13wt%, Ni: 1.66-4.11wt%, Ti: 1.36-3.35wt%, and Mo: 2.72-6.72wt%, and the high entropy alloy mixture is prepared by high energy ball milling;

[0011] (2) Preparation of (Ti,M)(C,N) ceramic solid solution powder: TiC, TiN, Mo 2 C.Cr3 C 2 , VC, and TaC are used as raw materials to prepare a mixture with the following mass percentages: Ti: 6.23-7.20wt%, Mo: 11.52-15.28wt%, Cr: 9.37-12.43wt%, V: 3.06-4.06wt%, Ta: 10.86-14.42wt%, C: 4.33-5.74wt%, and N: 0.94-1.03wt%, and a (Ti, M) (C, N) ceramic solid solution powder mixture is prepared by high-energy ball milling;

[0012] (3) Preparation of wet-grinded mixed material: The two mixed materials obtained in step (1) and step (2) were mixed and wet-grinded in a ball mill for 12 to 16 hours to obtain an intermediate wet-grinded mixed material, and then TiO 2 Add the graphite powder to the intermediate wet-milled mixture and continue ball milling for 8 to 10 hours to finally obtain a mixed metal-ceramic slurry;

[0013] (4) drying the mixed slurry obtained in step (3), adding a molding agent, pressing and sintering, to obtain the high entropy (Ti, M) (C, N)-based cermet having a twin crystal structure;

[0014] Furthermore, the high-energy ball milling in the above step (1) is carried out in a planetary ball mill, the ball milling process is dry milling, the grinding balls are cemented carbide balls with a diameter of 5 mm, the ball-to-material ratio is 15:1-30:1, the ball milling speed is 300-400 rpm, the ball milling time is 10-15 h, and the ball milling is carried out in an Ar atmosphere throughout the process, and the Ar pressure in the ball mill tank is 0.4-0.6 atm;

[0015] Furthermore, the high-energy ball milling in the above step (2) is carried out in a planetary ball mill, the ball milling process is dry milling, the grinding balls are cemented carbide balls with a diameter of 8 mm, the ball-to-material ratio is 10:1-20:1, the ball milling speed is 350-450 rpm, the ball milling time is 8-14 h, and the whole ball milling is carried out under Ar atmosphere, and the argon pressure in the ball mill tank is 0.4-0.6 atm;

[0016] Furthermore, the intermediate wet-milled mixture of the above step (3) is prepared in a planetary ball mill, the grinding balls are 30% of 10 mm diameter cemented carbide balls, 30% of 8 mm diameter cemented carbide balls and 40% of 5 mm diameter cemented carbide balls, the ball-to-material ratio is 5:1-7:1, the ball milling speed is 200-280 rpm, the ball milling time is 12-16 h, and the wet milling medium is anhydrous ethanol, and the addition amount thereof is preferably 2.0-2.5 times the weight of the mixture; when TiO 2After graphite powder was added to the intermediate wet grinding mixture, the amount of cemented carbide balls and anhydrous ethanol in the ball mill jar no longer increased;

[0017] Furthermore, the drying in the above step (4) refers to drying in a far-infrared drying oven at a temperature of 70 to 90° C.; adding a molding agent refers to adding a polyethylene glycol aqueous solution at a concentration of 8 wt %, with a total addition ratio of 6 to 8 wt % of the mixture;

[0018] Furthermore, the compression molding in the above step (4) refers to bidirectional compression on a tablet press at a pressure of 240 to 300 MPa.

[0019] Furthermore, the sintering process in step (4) is mainly divided into five stages: in the first stage, the temperature is increased to 400-600°C, the heating rate is 0.4-0.6°C / min, and the temperature is kept for 1-3h; in the second stage, the temperature is increased to 1000-1250°C, the heating rate is 0.5-1°C / min, and the temperature is kept for 2-4h; in the third stage, the temperature is increased to 1280-1330°C, the heating rate is 1-2°C / min, and the temperature is kept for 0.5-1h; in the fourth stage, the temperature is increased to 1420-1480°C, the heating rate is 1-2°C / min, and the temperature is kept for 1-2h; the first four stages are vacuum sintering, and the vacuum degree in the furnace needs to be always maintained at 1.0×10 -1 ~1.0×10 -2 Pa; in the fifth stage, after the highest temperature insulation is completed, the vacuum pump is turned off, and Ar gas with a pressure of 2-4 atm is introduced into the furnace until the temperature drops to 1000℃, then the vacuum pump is turned on and cooled with the furnace.

[0020] To achieve this purpose, in the above step (1), a high entropy alloy binder phase is directly prepared by high-energy ball milling of metal powder, which causes a large number of crystal defects to be generated in the binder phase alloy powder during the ball milling process, which is beneficial to improving the sintering characteristics of the subsequent powder, reducing the liquidus point and further reducing the sintering temperature; at the same time, due to the formation of the high entropy alloy binder phase, the diffusion of metal elements is slowed down, and the dissolution-precipitation phenomenon of the hard phase in the binder phase is also correspondingly suppressed, which makes the fine hard phase particles prepared by in-situ carbon thermal reduction sintering more retained, and coexist with a large amount of coarse (Ti, M) (C, N) hard phase prepared by high-energy ball milling, and finally form a twin crystal structure.

[0021] To achieve this purpose, in the above step (2), multiple metal carbides are subjected to high-energy ball milling with TiN and TiC to prepare (Ti, M) (C, N) ceramic solid solution powder. The main reason is that through high-energy ball milling, various carbides can be more evenly mixed and dissolved together. The high-density defects and high specific surface energy generated during the high-energy ball milling process can greatly reduce the diffusion activation energy of the system, expand the solid solubility of each metal element in the carbide, so that the hard phase of this multi-alloy component can remain stable during the sintering process, and finally form a coreless / weak core structure hard phase with lower interfacial stress. In addition, due to the flattening effect of high-energy ball milling, the (Ti, M) (C, N) hard phase will have obvious plate-like characteristics. In addition, in the mixed wet milling process of step (3), the high entropy alloy and the (Ti, M) (C, N) ceramic solid solution powder are first mixed and ball milled to obtain an intermediate wet milled mixture, and then fine TiO is added again. 2 The purpose of ball milling with graphite powder is to reduce the uniform distribution between coarse and fine hard phase powders so that the TiO 2 The fine hard phase particles generated by in-situ carbothermal reduction can form a small aggregation area, and more fine particles can be retained in the subsequent sintering process, which is conducive to the formation of a twin-crystal hard phase structure.

[0022] To achieve this goal, vacuum sintering is divided into four stages. In the first stage, the temperature is raised to 400-600°C, the heating rate is 0.4-0.6°C / min, and the temperature is kept for 1-3 hours. This stage is the stage of removing the molding agent. The slow heating and long-term heat preservation are to completely remove the molding agent between the powders, thereby eliminating the influence on the subsequent sintering process; the second stage is heated to 1000-1250°C, the heating rate is 0.5-1°C / min, and the temperature is kept for 2-4 hours. In this stage, the fine particles of TiO 2In a vacuum sintering furnace, an in-situ carbon thermal reduction reaction with graphite powder occurs to generate TiC, and solid solution is formed with free TiN powder in the powder to generate fine particles of Ti(C,N) hard phase. The CO released during the reduction process can remove the adsorbed oxygen on the surface of the powder more thoroughly, purify the interface between the bonding phase and the hard phase, and enhance the bonding force. This makes the interface bonding strength between the fine particle hard phase and the bonding phase relatively higher, which is beneficial to improving the strength and toughness of the material. In the third stage, the temperature is raised to 1280-1330℃, the heating rate is 1-2℃ / min, and the temperature is kept for 0.5-1h. This stage is the solid phase reaction stage, and the element diffusion between the hard phase and the bonding phase and the bonding between the powder particles mainly occur. Due to the difference in the hard phase composition of coarse and fine particles, the fine particle hard phase is more likely to diffuse with the alloy elements in the bonding phase, thereby forming a core-ring structure or (Ti,M)(C,N) white core particles, while the coarse particles have obvious high entropy effect due to the effect of high-energy ball milling. As a result, the diffusion of elements during the sintering process is slow, so most of the particles are coreless. In addition, due to the high entropy of the metal powder, some liquid phase will appear in this stage to partially fill the pores between the powders, which can greatly increase the density of the sintered body in the solid phase reaction stage. The fourth stage is heated to 1420-1480°C, with a heating rate of 1-2°C / min and insulation for 1-2h. This stage is the final sintering stage of the metal ceramic. The liquid phase completes a large amount of filling of the pores of the sintered body and further rearranges the particles to complete the densification of the sintered body, and finally forms a metal ceramic with a twin crystal structure. In the fifth stage, after the highest temperature insulation is completed, the vacuum pump is turned off, and Ar gas with a pressure of 2-4atm is introduced into the furnace until the temperature drops to 1000°C, then the vacuum pump is turned on and cooled with the furnace. The purpose is to prevent the fine hard phase in the microstructure from staying in the liquid phase for too long and merging and growing. It can refine the ceramic phase particles to a certain extent and maintain the bimodal characteristics of the metal ceramic hard phase particles. Finally, a high-entropy (Ti, M) (C, N)-based cermet with a twin-crystal structure of hard phase particles is obtained. Due to the coarse and fine combination of the microstructure, the cermet has both high hardness after fine-grain strengthening and the passivation, deflection and barrier effect of coarse-grained particles on cracks, thereby increasing the fracture toughness of the material. Finally, the twin-crystal structure high-entropy (Ti, M) (C, N)-based cermet has good comprehensive mechanical properties.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The high-entropy (Ti, M) (C, N)-based cermet with a twin crystal structure provided by the present invention has significantly higher hardness and toughness than cermets prepared by traditional methods. The high-entropy alloy binder phase and coarse-grained (Ti, M) (C, N) solid solution are directly prepared by high-energy ball milling, which greatly improves the sintering activity and reduces the sintering temperature.

[0025] 2. In the preparation process of the present invention, the hard phase is generated in situ in two different ways, so that the combination of the coarse-grained or fine-grained hard phase and the binding phase is tighter and the interface stress is lower, which improves the strength and toughness of the material while maintaining the high hardness of the metal ceramic.

[0026] 3. The sintering process of the present invention is carried out under only one thermal cycle condition, the process is simple, and an ordinary vacuum sintering furnace can meet the production requirements, which is conducive to industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the SEM microstructure image of the high entropy (Ti, M) (C, N) based metal ceramic with a twin crystal structure prepared in Example 1.

[0028] Figure 2 This is the grain size distribution diagram of the high entropy (Ti, M) (C, N)-based metal ceramic with a twin crystal structure prepared in Example 1. DETAILED DESCRIPTION

[0029] The following examples further illustrate the technical effects of the present invention. The raw materials used in the following examples are Fe powder, Co powder, Ni powder, Ti powder, Mo powder, TiO 2 Powder, TiC powder, TiN powder, Mo 2 C powder, Cr 3 C 2 Powder, VC powder, TaC powder and graphite powder; wherein the particle size of the single metal powder is 2-4 μm, the particle size of the metal carbide powder is 3-6 μm, the particle size of the graphite powder is 1-2 μm, and the particle size of the TiO 2 The particle size of the powder is 0.2-0.5 μm;

[0030] Table 1 shows the composition of the high entropy alloy mixture with four component formulas, Table 2 shows the composition of the (Ti, M) (C, N) ceramic solid solution powder with four component formulas, and Table 3 shows the composition of the TiO 2 and graphite powder. The three different process parameters of Examples 1-3 were used to prepare metal ceramics, and the Rockwell hardness, flexural strength and fracture toughness of the samples were measured. The following Rockwell hardness was measured according to GB / T 3849.1-2015 standard, the room temperature flexural strength was measured according to GB / T 3851-2015 standard, and the fracture toughness was measured according to GB / T33819-2017 standard.

[0031] Table 1 Composition of high entropy alloy mixtures of four composition formulas of metal ceramics (wt%)

[0032] Table 2 Composition of (Ti, M) (C, N) ceramic solid solution powders of four composition formula metal ceramics (wt%)

[0033]

[0034] Table 3 TiO in four composition formulas of cermets 2 and graphite powder composition (wt%)

[0035]

[0036] Example 1

[0037] 1. Preparation of high entropy alloy mixtures: Fe, Co, Ni, Ti, and Mo were used as raw materials. Four kinds of high entropy alloy mixtures were prepared according to Table 1, and placed in a planetary ball mill for high-energy ball milling. The grinding balls were 5 mm in diameter cemented carbide balls, the ball-to-material ratio was 20:1, the ball milling speed was 300 rpm, the ball milling time was 12 h, and the ball milling was carried out under Ar atmosphere throughout the process. The Ar pressure in the ball mill was 0.4 atm.

[0038] 2. Preparation of (Ti, M) (C, N) ceramic solid solution powder: TiC, TiN, Mo 2 C.Cr 3 C 2 , VC, and TaC were used as raw materials. Four kinds of (Ti, M) (C, N) ceramic solid solution powders were prepared according to Table 2 and placed in a planetary ball mill for high-energy ball milling. The grinding balls were 8 mm in diameter cemented carbide balls, the ball-to-material ratio was 10:1, the ball milling speed was 400 rpm, the ball milling time was 14 h, and the whole ball milling process was carried out under Ar atmosphere. The argon pressure in the ball mill was 0.4 atm.

[0039] 3. Preparation of wet-milled mixture: The mixtures prepared in step 1 and step 2 were mixed and wet-milled in a ball mill for 12 h to obtain an intermediate wet-milled mixture. The wet-milling was carried out in a planetary ball mill. The grinding balls were 30% carbide balls with a diameter of 10 mm, 30% carbide balls with a diameter of 8 mm, and 40% carbide balls with a diameter of 5 mm. The ball-to-material ratio was 6:1. The ball milling speed was 200 rpm. The wet-milling medium was anhydrous ethanol, and the amount thereof added was preferably 2.2 times the weight of the mixture. Subsequently, different proportions of TiO 2 The intermediate wet-milled mixtures of the four component formulas were added with graphite powder and ball milled for 10 h to finally obtain a mixed metal-ceramic slurry;

[0040] 4. Drying: drying the metal-ceramic slurry obtained in step 3 in a far-infrared drying oven at a drying temperature of 80° C. to obtain a metal-ceramic mixed powder;

[0041] 5. Adding a molding agent: Add a molding agent to the mixed powder obtained in step 4. The molding agent is a polyethylene glycol aqueous solution with a concentration of 8wt.%, and the addition ratio is 6wt% of the mixed material;

[0042] 6. Pressing molding: The pressure used for pressing molding is 300MPa;

[0043] 7. Sintering: It is carried out in a vacuum / atmosphere integrated furnace. First, the sintering furnace with the green body is heated to 500°C at a heating rate of 0.4°C / min and kept at this temperature for 2 hours; then the temperature is raised to 1000°C at a heating rate of 0.5°C / min and kept at this temperature for 4 hours; then the temperature is raised to 1300°C at a heating rate of 2°C / min and kept at this temperature for 1 hour; then the temperature is raised to 1450°C at a heating rate of 1°C / min and kept at this temperature for 1 hour; the above sintering processes are all carried out in a vacuum degree of 1.0×10 -1 ~1.0×10 -2 Pa; finally, after the highest temperature insulation is completed, the vacuum pump is turned off, and Ar gas with a pressure of 2 atm is introduced into the furnace until the temperature drops to 1000℃, then the vacuum pump is turned on and cooled with the furnace.

[0044] Under the above preparation process conditions, the mechanical properties of metal ceramics prepared with different component ratios are shown in Table 4.

[0045] Table 4 Mechanical properties of different metal ceramics prepared in Example 1

[0046] Figure 1 This is the SEM microstructure of the high entropy (Ti, M) (C, N) based cermet with a twin crystal structure prepared in this embodiment. Figure 2 This is a grain size distribution diagram of the high entropy (Ti, M) (C, N) based metal ceramic with a twin crystal structure prepared in this embodiment. It can be clearly seen from the figure that the prepared high entropy (Ti, M) (C, N) based metal ceramic has an obvious twin crystal structure grain size distribution.

[0047] Example 2

[0048] The steps for preparing the metal ceramic in this embodiment are as follows:

[0049] 1. Preparation of high entropy alloy mixtures: Fe, Co, Ni, Ti, and Mo were used as raw materials. Four kinds of high entropy alloy mixtures were prepared according to Table 1, and placed in a planetary ball mill for high-energy ball milling. The grinding balls were 5 mm in diameter cemented carbide balls, the ball-to-material ratio was 30:1, the ball milling speed was 330 rpm, the ball milling time was 10 h, and the ball milling was carried out under Ar atmosphere throughout the process. The Ar pressure in the ball mill was 0.6 atm.

[0050] 2. Preparation of (Ti, M) (C, N) ceramic solid solution powder: TiC, TiN, Mo 2 C.Cr 3 C 2 , VC, TaC as raw materials, four kinds of (Ti, M) (C, N) ceramic solid solution powders were prepared according to Table 2, and placed in a planetary ball mill for high-energy ball milling. The grinding balls were 8 mm in diameter cemented carbide balls, the ball-to-material ratio was 16:1, the ball milling speed was 350 rpm, the ball milling time was 12 h, and the whole ball milling process was carried out under Ar atmosphere, and the argon pressure in the ball mill was 0.5 atm;

[0051] 3. Preparation of wet-milled mixture: The mixtures prepared in step 1 and step 2 were mixed and wet-milled in a ball mill for 16 hours to obtain an intermediate wet-milled mixture. The wet-milling was carried out in a planetary ball mill. The grinding balls were 30% carbide balls with a diameter of 10 mm, 30% carbide balls with a diameter of 8 mm and 40% carbide balls with a diameter of 5 mm. The ball-to-material ratio was 5:1. The ball milling speed was 280 rpm. The wet-milling medium was anhydrous ethanol, and the amount thereof added was preferably 2.0 times the weight of the mixture. Subsequently, different proportions of TiO 2 The intermediate wet-milled mixtures of the four component formulas were added with graphite powder and ball milled for 8 h to obtain a mixed metal-ceramic slurry.

[0052] 4. Drying: drying the metal-ceramic slurry obtained in step 3 in a far-infrared drying oven at a drying temperature of 70° C. to obtain a metal-ceramic mixed powder;

[0053] 5. Adding a molding agent: Add a molding agent to the mixed powder obtained in step 4. The molding agent is a polyethylene glycol aqueous solution with a concentration of 8wt.%, and the addition ratio is 8wt% of the mixed material;

[0054] 6. Pressing and molding: The pressure used for pressing and molding is 240MPa;

[0055] 7. Sintering: It is carried out in a vacuum / atmosphere integrated furnace. First, the sintering furnace with the green body is heated to 400°C at a heating rate of 0.5°C / min and kept at this temperature for 3 hours; then the temperature is raised to 1200°C at a heating rate of 0.7°C / min and kept at this temperature for 3 hours; then the temperature is raised to 1330°C at a heating rate of 1.5°C / min and kept at this temperature for 0.8 hours; then the temperature is raised to 1420°C at a heating rate of 2°C / min and kept at this temperature for 2 hours; the above sintering processes are all carried out in a vacuum degree of 1.0×10 -1 ~1.0×10 -2 Pa; finally, after the highest temperature insulation is completed, the vacuum pump is turned off, and Ar gas with a pressure of 4 atm is introduced into the furnace until the temperature drops to 1000℃, then the vacuum pump is turned on and cooled with the furnace.

[0056] Under the above preparation process conditions, the mechanical properties of metal ceramics prepared with different component ratios are shown in Table 5.

[0057] Table 5 Mechanical properties of different metal ceramics prepared in Example 2

[0058] Example 3

[0059] The steps for preparing the metal ceramic in this embodiment are as follows:

[0060] 1. Preparation of high entropy alloy mixtures: Fe, Co, Ni, Ti, and Mo were used as raw materials. Four kinds of high entropy alloy mixtures were prepared according to Table 1, and placed in a planetary ball mill for high-energy ball milling. The grinding balls were 5 mm in diameter cemented carbide balls, the ball-to-material ratio was 15:1, the ball milling speed was 400 rpm, the ball milling time was 15 h, and the ball milling was carried out under Ar atmosphere throughout the process. The Ar pressure in the ball mill was 0.5 atm.

[0061] 2. Preparation of (Ti, M) (C, N) ceramic solid solution powder: TiC, TiN, Mo 2 C.Cr 3 C 2 , VC, and TaC were used as raw materials. Four kinds of (Ti, M) (C, N) ceramic solid solution powders were prepared according to Table 2 and placed in a planetary ball mill for high-energy ball milling. The grinding balls were 8 mm in diameter cemented carbide balls, the ball-to-material ratio was 20:1, the ball milling speed was 450 rpm, the ball milling time was 8 h, and the ball milling was carried out under Ar atmosphere. The argon pressure in the ball mill was 0.6 atm.

[0062] 3. Preparation of wet-milled mixture: The mixtures prepared in step 1 and step 2 were mixed and wet-milled in a ball mill for 14 h to obtain an intermediate wet-milled mixture. The wet-milling was carried out in a planetary ball mill. The grinding balls were 30% carbide balls with a diameter of 10 mm, 30% carbide balls with a diameter of 8 mm, and 40% carbide balls with a diameter of 5 mm. The ball-to-material ratio was 7:1. The ball milling speed was 240 rpm. The wet-milling medium was anhydrous ethanol, and the amount thereof added was preferably 2.5 times the weight of the mixture. Subsequently, different proportions of TiO 2 The intermediate wet-milled mixtures of the four component formulas were added with graphite powder and ball milled for 9 h to obtain a mixed metal-ceramic slurry.

[0063] 4. Drying: drying the metal-ceramic slurry obtained in step 3 in a far-infrared drying oven at a drying temperature of 90° C. to obtain a metal-ceramic mixed powder;

[0064] 5. Adding a molding agent: Add a molding agent to the mixed powder obtained in step 4. The molding agent is a polyethylene glycol aqueous solution with a concentration of 8wt.%, and the addition ratio is 7wt% of the mixed material;

[0065] 6. Pressing molding: The pressure used for pressing molding is 260MPa;

[0066] 7. Sintering: It is carried out in a vacuum / atmosphere integrated furnace. First, the sintering furnace with the green body is heated to 600℃, the heating rate is 0.6℃ / min, and the temperature is kept for 4h; then the temperature is raised to 1250℃, the heating rate is 1℃ / min, and the temperature is kept for 2h; then the temperature is raised to 1280℃, the heating rate is 1℃ / min, and the temperature is kept for 0.5h; then the temperature is raised to 1480℃, the heating rate is 1.5℃ / min, and the temperature is kept for 1.5h; the above sintering processes are all carried out in a vacuum degree of 1.0×10 -1 ~1.0×10 -2 Pa; finally, after the highest temperature is maintained, the vacuum pump is turned off, and Ar gas with a pressure of 3 atm is introduced into the furnace until the temperature drops to 1000℃, then the vacuum pump is turned on and the furnace is cooled. Under the above preparation process conditions, the mechanical properties of metal ceramics prepared with different component ratios are shown in Table 6.

[0067] Table 6 Mechanical properties of different metal ceramics prepared in Example 3

[0068] Within the value range of the claims, the synthesis parameters of high entropy alloy powder, the ball milling mixing parameters of hard phase powder, and the process parameters such as the heating rate and holding time during the sintering process have a relatively large influence on the microstructure and mechanical properties of high entropy metal ceramics. Only when the sintering temperature and holding time of this stage are reasonably matched, the carbon thermal reduction process and liquid phase sintering process of the above stage can be reasonably and fully carried out to prepare a twin-crystal structure high entropy (Ti, M) (C, N)-based metal ceramic with better comprehensive mechanical properties. Within the value range of the claims, its influence on the mechanical properties of the material is limited.

[0069] The above embodiments are only used to illustrate the contents of the present invention rather than to limit the present invention. Therefore, any changes within the meaning and scope equivalent to the claims of the present invention should be considered to be included in the scope of the claims.

[0070] The present invention has many specific application paths. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements can be made without departing from the principle of the present invention. These improvements should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a twin-crystal structure high entropy (Ti, M) (C, N)-based cermet, characterized in that: The metal ceramic is prepared from high entropy alloy powder, (Ti, M) (C, N) ceramic solid solution powder prepared by high-energy ball milling, TiO2 and graphite powder as raw materials, M is four elements of Mo, Cr, V and Ta, and the metal ceramic microstructure prepared after sintering is composed of hard phase particles with obvious bimodal distribution and high entropy alloy matrix bonding phase uniformly distributed; The raw materials of the metal ceramic are composed of the following mass percentages: Fe: 1.58-3.91wt%, Co: 1.67-4.13wt%, Ni: 1.66-4.11wt%, Ti: 21.27-22.51wt%, Mo: 18.00-18.24wt%, Cr: 9.37-12.43wt%, V: 3.06-4.06wt%, Ta: 10.86-14.42wt%, O: 8.50-8.65wt%, C: 14.18-15.42wt%, N: 0.94-1.03wt%; In the composition of the metal ceramic, the high entropy alloy binder phase is introduced by Fe, Co, Ni, Ti, and Mo single metal powders, C is introduced by various metal carbide powders and graphite powder, N is introduced by TiN, and O is introduced by TiO2; wherein the particle size of the single metal powder is 2 to 4 μm, the particle size of the metal carbide powder is 3 to 6 μm, the particle size of the graphite powder is 1 to 2 μm, and the particle size of the TiO2 powder is 0.2 to 0.5 μm; The method for preparing the metal ceramic further comprises the following steps: (1) Preparation of high entropy alloy mixture A mixture of Fe, Co, Ni, Ti and Mo is prepared as raw materials with the following weight percentages: Fe: 1.58-3.91wt%, Co: 1.67-4.13wt%, Ni: 1.66-4.11wt%, Ti: 1.36-3.35wt%, Mo: 2.72-6.72wt%, and a high entropy alloy mixture is prepared by high-energy ball milling; (2) Preparation of (Ti, M) (C, N) ceramic solid solution powder A mixture of TiC, TiN, Mo2C, Cr3C2, VC and TaC with mass percentages of: Ti: 6.23-7.20wt%, Mo: 11.52-15.28wt%, Cr: 9.37-12.43wt%, V: 3.06-4.06wt%, Ta: 10.86-14.42wt%, C: 4.33-5.74wt%, and N: 0.94-1.03wt% is prepared by high-energy ball milling to prepare a (Ti, M) (C, N) ceramic solid solution powder mixture; (3) Preparation of wet-milled mixture: The two mixtures prepared in step (1) and step (2) are mixed and wet-milled in a ball mill for 12 to 16 hours to obtain an intermediate wet-milled mixture, and then TiO2 and graphite powder with a mass percentage of Ti: 12.71 to 12.93wt%, O: 8.50 to 8.65wt%, and C: 9.68 to 9.85wt% are added to the intermediate wet-milled mixture and the ball milling is continued for 8 to 10 hours to finally obtain a mixed metal ceramic slurry; (4) The mixed slurry obtained in step (3) is dried, a molding agent is added, pressed and sintered to obtain a high entropy (Ti, M) (C, N)-based metal ceramic with a twin crystal structure.

2. The method for preparing a twin-crystal high-entropy (Ti, M) (C, N)-based cermet according to claim 1, characterized in that: The high-energy ball milling in step (1) is carried out in a planetary ball mill. The ball milling process is dry milling. The grinding balls are cemented carbide balls with a diameter of 5 mm. The ball-to-material ratio is 15:1 to 30:

1. The ball milling speed is 300 to 400 rpm. The ball milling time is 10 to 15 hours. The whole ball milling process is carried out under Ar atmosphere. The Ar pressure in the ball mill tank is 0.4 to 0.6 atm.

3. The method for preparing a twin-crystal high-entropy (Ti, M) (C, N)-based cermet according to claim 1, characterized in that: The high-energy ball milling in step (2) is carried out in a planetary ball mill. The ball milling process is dry milling. The grinding balls are cemented carbide balls with a diameter of 8 mm. The ball-to-material ratio is 10:1-20:

1. The ball milling speed is 350-450 rpm. The ball milling time is 8-14 h. The entire ball milling process is carried out under Ar atmosphere. The argon pressure in the ball mill is 0.4-0.6 atm.

4. The method for preparing a twin-crystal high-entropy (Ti, M) (C, N)-based cermet according to claim 1, characterized in that: The preparation of the intermediate wet-milled mixture in the step (3) is carried out in a planetary ball mill, the grinding balls are 30% of carbide balls with a diameter of 10 mm, 30% of carbide balls with a diameter of 8 mm and 40% of carbide balls with a diameter of 5 mm, the ball-to-material ratio is 5:1-7:1, the ball milling speed is 200-280 rpm, the ball milling time is 12-16 h, and the wet milling medium is anhydrous ethanol, the amount of which is 2.0-2.5 times the weight of the mixture; after TiO2 and graphite powder are added to the intermediate wet-milled mixture, the amount of carbide balls and anhydrous ethanol in the ball mill jar no longer increases.

5. The method for preparing a twin-crystal structure high entropy (Ti, M) (C, N)-based cermet according to claim 1, characterized in that: The drying in step (4) refers to drying in a far-infrared drying oven at a temperature of 70 to 90° C.; adding a molding agent refers to adding a polyethylene glycol aqueous solution at a concentration of 8 wt %, with the total addition ratio being 6 to 8 wt % of the mixture.

6. The method for preparing a twin-crystal high-entropy (Ti, M) (C, N)-based cermet according to claim 1, characterized in that: The compression molding in step (4) refers to bidirectional compression on a tablet press at a pressure of 240 to 300 MPa.

7. The method for preparing a twin-crystal high-entropy (Ti, M) (C, N)-based cermet according to claim 1, characterized in that: The sintering process of step (4) is mainly divided into five stages: the first stage, heating to 400-600°C, heating rate of 0.4-0.6°C / min, and keeping warm for 1-3h; the second stage, heating to 1000-1250°C, heating rate of 0.5-1°C / min, and keeping warm for 2-4h; the third stage, heating to 1280-1330°C, heating rate of 1-2°C / min, and keeping warm for 0.5-1h; the fourth stage, heating to 1420-1480°C, heating rate of 1-2°C / min, and keeping warm for 1-2h; the first four stages are vacuum sintering, and the vacuum degree in the furnace needs to be always maintained at 1.0×10 -1 ~1.0×10 -2 Pa; in the fifth stage, after the highest temperature insulation is completed, the vacuum pump is turned off, and Ar gas with a pressure of 2-4 atm is introduced into the furnace until the temperature drops to 1000℃, then the vacuum pump is turned on and cooled with the furnace.