A growth method for improving the growth rate of silicon carbide single crystal by PVT method
By introducing CO partial pressure during the silicon carbide PVT growth process, the transport efficiency of carbon components in silicon carbide powder is improved, thus solving the problem of slow growth rate of silicon carbide single crystals and achieving improved crystal growth rate and reduced cost.
Patent Information
- Application Number
- CN202411089550.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing PVT method for growing silicon carbide single crystals has a slow growth rate, resulting in thinner ingots, longer growth cycles, higher costs, and insufficient production capacity.
Introducing CO partial pressure during the growth of silicon carbide PVT, using CO as a transport agent, and generating CO through high-temperature decomposition of high-melting-boiling-point solid oxides or by introducing oxygen-containing gas, improves the transport efficiency of carbon components in silicon carbide powder.
It improves the growth rate of silicon carbide single crystals, shortens the growth cycle, reduces costs, and increases crystal growth thickness and production capacity.
Smart Images

Figure CN118621432B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, and in particular to a growth method for improving the growth rate of silicon carbide single crystal using a PVT method. Background Art
[0002] Silicon carbide has excellent physical and chemical properties such as large bandgap, high breakdown electric field, good thermal conductivity, and fast saturated electron drift rate. It is a typical third-generation semiconductor material after silicon and gallium arsenide. It has very broad applications in high-temperature, high-frequency, high-power devices and deep ultraviolet optoelectronic devices, especially in the fields of electric vehicles (xEV), rail transit (Rail) and motor driving (Motordriving). Its share is rapidly increasing, so it is regarded as one of the most promising materials in the field of semiconductor materials.
[0003] At present, the mainstream growth method for commercial silicon carbide substrates is physical vapor transport (PVT), and its specific growth method is: place a seed crystal on the top of the crucible, add powder at the bottom of the crucible, place the crucible heat field in a crystal growth furnace, the bottom temperature of the crucible is high, and the top temperature is low. By controlling the temperature and pressure, the bottom powder gradually sublimates and is transferred to the top seed crystal for condensation and crystallization, thereby achieving the growth of silicon carbide single crystals. At present, this method has become the mainstream method in the industry and has achieved large-scale production.
[0004] However, the current PVT method for growing silicon carbide single crystals still has the problems of slow single crystal growth rate and short single crystal length. This is because silicon carbide sublimation is not based on stoichiometric ratios, and the sublimation atmosphere is rich in silicon, resulting in a large amount of carbon remaining at the bottom of the crucible. The sublimation atmosphere will have more silicon after condensation, and the excess silicon will reduce the growth rate of silicon carbide, corrode the graphite crucible, and introduce defects such as carbon inclusions. To solve this problem, the research team proposed the use of high melting and boiling point coatings such as tantalum carbide (TaC), tungsten carbide (WC), and niobium carbide (NbC), which can effectively improve the quality of crystal growth and reduce the generation of defects and dislocations. However, the application of the coating seriously hinders the crystal growth rate, prolongs the growth cycle (up to 15-20 days), and the thickness of the grown crystal ingot is relatively thin (only about 1-1.5cm can be sliced), which makes the cost of growing silicon carbide single crystals high. At the same time, the production capacity of application-grade silicon carbide substrates is seriously insufficient, which restricts the development of the silicon carbide industry.
[0005] In view of the problems of slow growth rate, unbalanced carbon-silicon ratio, thin ingot thickness, etc. during the growth of silicon carbide single crystal, the present invention provides a growth method for improving the growth rate of silicon carbide single crystal by PVT method. Summary of the invention
[0006] The purpose of the present invention is to provide a growth method for improving the growth rate of silicon carbide single crystals by the PVT method, so as to achieve the purpose of reducing costs and increasing efficiency by increasing the crystal growth rate, compressing the crystal growth cycle, reducing costs, increasing the crystal growth thickness, and increasing production capacity.
[0007] To achieve the above-mentioned object, the present invention provides a growth method for improving the growth rate of silicon carbide single crystal by PVT method, wherein CO partial pressure is introduced into the atmosphere during the silicon carbide PVT growth process, CO is used as a transmission agent, and the transmission efficiency of the carbon component in the silicon carbide powder is improved, thereby improving the growth rate of the silicon carbide single crystal.
[0008] Preferably, the method for introducing CO includes directly introducing CO or generating CO by reaction.
[0009] Preferably, the method for generating CO by reaction comprises adding a high melting point solid oxide or introducing an external gas.
[0010] Preferably, the high melting point solid oxide is one of silicon dioxide, zirconium oxide or tantalum oxide.
[0011] Preferably, the added gas is one of argon-oxygen mixed gas, helium-oxygen mixed gas, CO2, water vapor, ethanol, methanol, H2O2, ozone, and carbonic acid.
[0012] In the present invention, a small amount of high melting point solid oxide is added to high purity silicon carbide powder, which can decompose oxygen in the oxide at high temperature, so that it can react with the decomposing carbon-rich silicon carbide powder to produce CO.
[0013] When adding external gas, it is necessary to place carbon powder or graphite in the gas passage, and introduce a single gas containing the O element or a gasifiable substance, such as a mixture of rare gases such as O3, argon oxygen / helium oxygen and oxygen, through the gas duct. At high temperature, O3 or O2 reacts with high-purity carbon powder or graphite to generate CO.
[0014] When gasifiable compounds containing three or two elements of C, H, and O, such as CO2 and water vapor, are introduced, these compounds can directly react with high-purity carbon powder or graphite to generate CO. Among them, CO2 reacts with carbon at high temperature to generate CO; H2O reacts with carbon to generate CO and H2.
[0015] For example, oxygen-containing organic compounds such as ethanol, methanol, H2O2, and carbonic acid produce CO2 and H2O(g) or one of them at high temperature, and the produced CO2 and H2O(g) react with high-purity carbon powder or graphite to produce CO. Among them, ethanol and methanol produce CO at high temperature; H2O2 decomposes water vapor and oxygen at high temperature, and water vapor and oxygen react with carbon to produce CO; carbonic acid decomposes at high temperature to produce CO2 and water, which react with carbon to produce CO.
[0016] Therefore, the present invention provides a growth method for improving the growth rate of silicon carbide single crystals by the PVT method. Compared with the existing methods, the present invention solves the problems of slow growth rate, unbalanced carbon-silicon ratio, and thin ingot thickness during the growth of silicon carbide single crystals, improves the crystal growth rate, shortens the crystal growth cycle, reduces costs, increases crystal growth thickness, and increases production capacity.
[0017] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the structure of the device for growing silicon carbide single crystal by the PVT method of the present invention.
[0019] Reference Numbers
[0020] 1-upper heater; 2-lower heater; 3-crystal growth crucible; 4-insulation layer; 5-upper temperature measuring hole; 6-lower temperature measuring hole; 7-first filter crucible; 8-second filter crucible; 9-first gas guide hole; 10-second gas guide hole; 11-third gas guide hole; 12-argon gas inlet pipe; 13-external gas inlet pipe; 14-seed crystal; 15-high-purity silicon carbide powder. DETAILED DESCRIPTION
[0021] The present invention provides a growth method for improving the growth rate of silicon carbide single crystals by the PVT method. During the growth process of silicon carbide PVT, a certain CO partial pressure is introduced into the atmosphere, CO is used as a transmission agent, and the transmission efficiency of the carbon component in the silicon carbide powder is improved, thereby improving the growth rate of the silicon carbide single crystal. The principle is expressed by the following chemical formula:
[0022] Si 1+X C+2XCO→(1+X)SiC+XCO2.
[0023] In the present invention, the device used for growing silicon carbide single crystal is a high-purity graphite crucible thermal field, and the thermal field structure is as follows: Figure 1As shown, it includes an upper heater 1 and a lower heater 2 arranged below the upper heater 1, a crystal growth crucible 3 is arranged in the upper heater 1, and an insulation layer 4 is arranged around the upper heater 1 and the lower heater 2. An upper temperature measuring hole 5 is opened above the insulation layer 4, and a lower temperature measuring hole 6 is opened below the insulation layer 4. The insulation layer 4 is coaxially symmetrical with the upper and lower temperature measuring holes, the upper and lower heaters, and the crystal growth crucible 3. A first filter crucible 7 and a second filter crucible 8 are sequentially sleeved in the lower heater 2 from the outside to the inside, a first air guide hole 9 is opened at the bottom of the upper heater 1, a second air guide hole 10 is opened on the first filter crucible 7, and a third air guide hole 11 is opened on the second filter crucible 8. An argon gas inlet pipe 12 and an external gas inlet pipe 13 are opened at the bottom below the insulation layer 4. The external gas inlet pipe 13 is connected to the second filter crucible 8. There are two argon gas inlet pipes 12, which are respectively arranged on both sides of the lower temperature measuring hole 6 and are both connected to the lower heater 2.
[0024] In the present invention, the surfaces of the upper and lower heaters, the crystal growth crucible 3 and the first and second filter crucibles are coated with an oiled tantalum carbide coating. The two argon gas inlet pipes 12 are opened throughout the crystal growth process to form an isolation layer on the surface of the hot field. High-purity silicon carbide powder 15 is placed at the bottom of the crystal growth crucible 3, and the seed crystal 14 is located at the top of the crystal growth crucible 3.
[0025] In the present invention, the methods for introducing CO include the following:
[0026] (1) Adding a small amount of SiO2 to the high-purity silicon carbide powder in the crucible can decompose oxygen at high temperature, so that it can react with the carbon-rich silicon carbide powder being decomposed to produce CO; (2) Adding oxides such as zirconium oxide and tantalum oxide to the high-purity silicon carbide powder in the crucible can decompose oxygen at high temperature, so that it can react with the carbon-rich silicon carbide powder being decomposed to produce CO; (3) Directly introduce CO; (4) Introduce a mixture of rare gases such as argon oxygen / helium oxygen and oxygen, and place carbon powder or graphite in the gas passage, so that oxygen reacts with carbon at high temperature to produce CO; (5) Introduce CO2, and place carbon powder or graphite in the gas passage, so that CO 2 reacts with carbon at high temperature to generate CO; (6) water vapor is introduced and carbon powder or graphite is placed in the gas passage, so that H2O reacts with carbon to generate CO and H2; (7) oxygen-containing organic matter such as ethanol and methanol is introduced to decompose and generate CO; (8) H2O2 is introduced and carbon powder or graphite is placed in the gas passage, so that H2O2 decomposes water vapor and oxygen at high temperature, and the water vapor and oxygen react with carbon to generate CO; (9) ozone is introduced and carbon powder or graphite is placed in the gas passage, so that ozone reacts with carbon at high temperature to generate CO / CO2; (10) carbonic acid is introduced to decompose at high temperature to generate CO2 and water, which react with the carbon powder or graphite in the gas passage to generate CO.
[0027] When CO is introduced through a high melting point solid oxide, the specific steps are as follows:
[0028] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, add a small amount of high melting point solid oxide to the high purity silicon carbide powder 15 and mix evenly, place it at the bottom of the crystal growth crucible 3, tighten the crucible and place it in the upper heater 1.
[0029] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0030] Step 3: Set the temperature program under vacuum conditions, raise the temperature to 700-1450°C in 2-6 hours, then open the two argon inlet pipes 12 (gas flow rate is controlled at 1-5L / min), raise the pressure to 200-900mbar in 0.5-3 hours, and raise the temperature to 2000-2300°C in 2-6 hours under constant pressure of flowing argon, then reduce the pressure to the growth pressure (0.1-50mbar) within a certain period of time (0.5-50 hours). Grow under constant temperature flowing argon for 3-15 days.
[0031] Step 4: Before increasing the pressure and decreasing the temperature, keep the two argon gas inlet pipes 12 open (gas flow rate is controlled at 1-5 L / min), increase the pressure to 200-900 mbar for 0.5-3 hours, decrease the temperature to 700-1400°C in 10-20 hours, and then naturally decrease the temperature to complete the entire crystal growth.
[0032] When CO is generated by the reaction of the added gas, high-purity carbon powder or graphite is placed between the first filter crucible 7 and the second filter crucible 8. When the conditions required for growth are met, the external gas inlet pipe 13 is opened after a certain growth time or during the pressure reduction process, and a certain proportion of external gas is introduced. The first gas guide hole 9, the second gas guide hole 10 and the third gas guide hole 11 guide the generated CO into the crystal growth crucible 3.
[0033] The specific steps are as follows:
[0034] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0035] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0036] Step 3: Under vacuum conditions, set the temperature rising program, raise the temperature to 700-1450°C in 2-6 hours, then open the argon inlet pipe 12 (gas flow rate is controlled at 1-5L / min), increase the pressure to 200-900mbar in 0.5-3 hours, and under the condition of flowing argon constant pressure, raise the temperature to 2000-2300°C in 2-6 hours, and then reduce the pressure to the growth pressure (0.1-50mbar) within a certain period of time (0.5-50 hours). After a certain growth period or during the depressurization process, the external gas inlet pipe 13 is opened (the gas flow rate is controlled at 0-1000sccm, preferably controlled at 0-200sccm), and a certain proportion of external gas (high-purity CO / CO2, water vapor, anhydrous ethanol / methanol, ozone, hydrogen peroxide gas, carbonic acid gas, etc.) is introduced so that the Ar and CO partial pressure (Ar / CO) is controlled at: 3~4000:1 (preferably controlled in the range of 10-1000:1), and the growth is carried out for 3~15 days under constant temperature flowing argon conditions.
[0037] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is controlled at 1-5L / min). Increase the pressure to 200-900mbar for 0.5-3 hours, decrease the temperature to 700-1400℃ in 10-20 hours, and then naturally decrease the temperature. The entire crystal growth is completed.
[0038] The following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] This embodiment provides a growth method for increasing the growth rate of a silicon carbide single crystal by a PVT method, by adding SiO2 to form CO, specifically comprising the following steps:
[0041] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, add a small amount of SiO2 powder to the high-purity silicon carbide powder 15, mix evenly, place it at the bottom of the crystal growth crucible 3, tighten the crucible, and place it in the upper heater 1.
[0042] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0043] Step 3: Under vacuum conditions, set the heating program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, and then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0044] Step 4: Before increasing the pressure and decreasing the temperature, keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min), increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C for 15 hours, and then decrease the temperature naturally, and the entire crystal growth is completed.
[0045] Example 2
[0046] This embodiment provides a growth method for increasing the growth rate of a silicon carbide single crystal by a PVT method, by adding tantalum oxide to form CO, specifically comprising the following steps:
[0047] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, add a small amount of tantalum oxide powder to the high-purity silicon carbide powder 15, mix evenly, place it at the bottom of the crystal growth crucible 3, tighten the crucible, and place it in the upper heater 1.
[0048] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0049] Step 3: Under vacuum conditions, set the heating program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, and then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0050] Step 4: Before increasing the pressure and decreasing the temperature, keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min), increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C for 15 hours, and then decrease the temperature naturally, and the entire crystal growth is completed.
[0051] Example 3
[0052] This embodiment provides a growth method for increasing the growth rate of a silicon carbide single crystal by a PVT method, directly introducing high-purity CO gas, and specifically comprising the following steps:
[0053] The first step: place the glued seeds on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place the high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0054] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0055] Step 3: Under vacuum conditions, set the temperature rising program, raise the temperature to 1350°C in 3 hours, then open the two argon gas inlet pipes 12 (gas flow rate is 1L / min), raise the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, then open the gas inlet pipe 13, introduce CO at a gas flow rate of 0.10L / min, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0056] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min). Then, under constant temperature flowing argon conditions, increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C in 15 hours, and then naturally cool down to complete the entire crystal growth.
[0057] Example 4
[0058] This embodiment provides a growth method for improving the growth rate of a silicon carbide single crystal by a PVT method, wherein an argon-oxygen mixed gas is introduced to form CO, and specifically comprises the following steps:
[0059] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0060] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0061] Step 3: Under vacuum conditions, set the heating program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, then open the inlet pipe 13, and introduce argon-oxygen mixed gas (oxygen content <0.1%) at a gas flow rate of 0.1L / min, then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0062] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min). Increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C in 15 hours, and then cool naturally to complete the entire crystal growth.
[0063] Example 5
[0064] This embodiment provides a growth method for increasing the growth rate of a silicon carbide single crystal by a PVT method, wherein CO2 is introduced to form CO, and specifically comprises the following steps:
[0065] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0066] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0067] Step 3: Under vacuum conditions, set the heating program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, then open the inlet pipe 13, introduce CO2 at a gas flow rate of 0.1L / min, and then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0068] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min). Increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C in 15 hours, and then cool naturally to complete the entire crystal growth.
[0069] Example 6
[0070] This embodiment provides a growth method for increasing the growth rate of a silicon carbide single crystal by a PVT method, wherein water vapor is introduced to form CO, and specifically comprises the following steps:
[0071] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0072] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0073] Step 3: Under vacuum conditions, set the heating program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, then open the inlet pipe 13, and introduce water vapor at a gas flow rate of 0.1L / min, then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0074] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min). Increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C in 15 hours, and then cool naturally to complete the entire crystal growth.
[0075] Example 7
[0076] This embodiment provides a growth method for improving the growth rate of a silicon carbide single crystal by a PVT method, wherein ethanol is introduced to form CO, and specifically comprises the following steps:
[0077] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0078] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0079] Step 3: Under vacuum conditions, set the temperature rising program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), raise the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, then open the bubbler and the inlet pipe 13 to allow ethanol to be introduced in gas mode at a gas flow rate of 0.1L / min, then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0080] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min). Increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C in 15 hours, and then cool naturally to complete the entire crystal growth.
[0081] Example 8
[0082] This embodiment provides a growth method for increasing the growth rate of a silicon carbide single crystal by a PVT method, wherein H2O2 is introduced to form CO, and specifically comprises the following steps:
[0083] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0084] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0085] Step 3: Under vacuum conditions, set the temperature rising program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), raise the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, then open the bubbler and the inlet pipe 13 to allow H2O2 to flow in gas mode at a gas flow rate of 0.1L / min, then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0086] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min). Increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C in 15 hours, and then cool naturally to complete the entire crystal growth.
[0087] Example 9
[0088] This embodiment provides a growth method for increasing the growth rate of a silicon carbide single crystal by a PVT method, wherein ozone is introduced to form CO, and specifically comprises the following steps:
[0089] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0090] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0091] Step 3: Under vacuum conditions, set the heating program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), increase the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, then open the inlet pipe 13, introduce ozone at a gas flow rate of 0.1L / min, and then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystal grows for 5 days.
[0092] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min). Increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C in 15 hours, and then cool naturally to complete the entire crystal growth.
[0093] Example 10
[0094] This embodiment provides a growth method for improving the growth rate of a silicon carbide single crystal by a PVT method, wherein carbonic acid is introduced to form CO, and specifically comprises the following steps:
[0095] The first step: place the bonded seed crystal 14 on the top of the crystal growth crucible 3, place the high-purity silicon carbide powder 15 on the bottom of the crystal growth crucible 3, tighten the crucible, place it in the upper heater 1, and place high-purity carbon powder or graphite between the first filter crucible 7 and the second filter crucible 8.
[0096] Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs.
[0097] Step 3: Under vacuum conditions, set the temperature rising program, raise the temperature to 1350°C in 3 hours, then open the two argon inlet pipes 12 (gas flow rate is 1L / min), raise the pressure to 300mbar in 1 hour, under the condition of flowing argon constant pressure, raise the temperature to 2100°C in 3 hours, then open the bubbler and the inlet pipe 13 to allow carbonic acid to be introduced in gas mode at a gas flow rate of 0.1L / min, then under the condition of constant temperature flowing argon, reduce the pressure to 5mbar in 1 hour, under the growth conditions of temperature: 2100°C, pressure: 5mbr, the crystals grow for 5 days.
[0098] Step 4: Before increasing the pressure and decreasing the temperature, close the external gas inlet pipe 13 and keep the two argon gas inlet pipes 12 open (gas flow rate is 1 L / min). Increase the pressure to 800 mbar for 1 hour, decrease the temperature to 1100°C in 15 hours, and then cool naturally to complete the entire crystal growth.
[0099] The control group was composed of silicon carbide powder without any additives.
[0100] The crystal growth rate and thickness of Examples 1-10 and the control group were experimentally tested, and the results are shown in Table 1.
[0101] Table 1
[0102] ;
[0103] As can be seen from Table 1, the present invention provides a growth method for improving the growth rate of silicon carbide single crystals by the PVT method, which improves the crystal growth rate, shortens the crystal growth cycle, reduces the cost, increases the crystal growth thickness, and increases the production capacity.
[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for increasing the growth rate of silicon carbide single crystals by PVT method, characterized in that: The specific steps are as follows: Step 1: Place the glued seed crystal on the top of the crystal growth crucible, add high melting point and boiling point solid oxide to the high purity silicon carbide powder, mix evenly, place it on the bottom of the crystal growth crucible, tighten the crucible and place it in the upper heater; Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs; Step 3: Under vacuum conditions, set the temperature program, raise the temperature to 700-1450°C in 2-6 hours, then open the two argon inlet pipes, control the gas flow rate at 1-5L / min, increase the pressure to 200-900mbar in 0.5-3 hours, and raise the temperature to 2000-2300°C under the condition of flowing argon constant pressure in 2-6 hours, then reduce the pressure to the growth pressure of 0.1-50mbar in 0.5-50 hours, and grow for 3-15 days under the condition of constant temperature flowing argon; Step 4: Before increasing the pressure and cooling down, keep the two argon gas inlet pipes open, control the gas flow rate at 1-5L / min, increase the pressure to 200-900mbar for 0.5-3 hours, cool down to 700-1400℃ in 10-20 hours, and then cool down naturally, and the entire crystal growth is completed; The surfaces of the upper heater and the crystal growth crucible are coated with tantalum carbide coating; The high melting and boiling point solid oxide is one of silicon dioxide, zirconium oxide or tantalum oxide; Adding high melting and boiling point solid oxides to high-purity silicon carbide powder can decompose the oxygen in the oxide at high temperature, so that it can react with the decomposing carbon-rich silicon carbide powder to produce CO. During the growth process of silicon carbide PVT, a certain CO partial pressure is introduced into the atmosphere. CO is used as a transmission agent to improve the transmission efficiency of the carbon component in the silicon carbide powder, thereby increasing the growth rate of silicon carbide single crystals. The principle is expressed by the following chemical formula: Si 1+X C+2XCO→(1+X)SiC+XCO2。 2. A method for increasing the growth rate of silicon carbide single crystals by PVT method, characterized in that: The specific steps are as follows: The first step: placing the bonded seed crystal on the top of the crystal growth crucible, placing the high-purity silicon carbide powder on the bottom of the crystal growth crucible, tightening the crucible, placing it in the upper heater, and placing the high-purity carbon powder or graphite between the first filter crucible and the second filter crucible; Step 2: After the furnace is loaded, the single crystal growth furnace is vacuumed to make the pressure inside the furnace reach 10 -6 mbar, set the corresponding temperature and pressure control programs; Step 3: Under vacuum conditions, set the temperature program, raise the temperature to 700-1450℃ in 2-6 hours, then open the argon gas inlet pipe, control the gas flow rate at 1-5L / min, increase the pressure to 200-900mbar in 0.5-3 hours, and under the condition of constant pressure of flowing argon, raise the temperature to 2000-2300℃ in 2-6 hours, and then reduce the pressure to the growth pressure of 0.1-50mbar in 0.5-50 hours; after a certain growth time or during the decompression process, open the additional gas inlet pipe, control the gas flow rate at 0-1000sccm, and introduce a certain proportion of additional gas to control the Ar and CO partial pressure at 3-4000:1, and grow for 3-15 days under constant temperature flowing argon conditions; Step 4: Before increasing the pressure and cooling down, close the external gas inlet pipe, keep the two argon gas inlet pipes open, control the gas flow rate at 1-5L / min, increase the pressure to 200-900mbar for 0.5-3 hours, cool down to 700-1400℃ in 10-20 hours, and then cool down naturally, and the entire crystal growth is completed; The added gas is one of high-purity CO / CO2, water vapor, anhydrous ethanol / methanol, ozone, hydrogen peroxide gas, carbon dioxide gas, argon-oxygen mixed gas, and helium-oxygen mixed gas; The device used for growing silicon carbide single crystal is a high-purity graphite crucible thermal field, the thermal field structure includes an upper heater and a lower heater arranged below the upper heater, a crystal growth crucible is arranged in the upper heater, and a thermal insulation layer is arranged around the upper heater and the lower heater, an upper temperature measuring hole is opened above the thermal insulation layer, and a lower temperature measuring hole is opened below the thermal insulation layer, and the thermal insulation layer and the upper and lower temperature measuring holes, the upper and lower heaters, and the crystal growth crucible are coaxially symmetrically arranged, and a first filter crucible and a second filter crucible are sequentially sleeved in the lower heater from the outside to the inside, a first air guide hole is opened at the bottom of the upper heater, a second air guide hole is opened on the first filter crucible, and a third air guide hole is opened on the second filter crucible, an argon gas inlet pipe and an external gas inlet pipe are opened at the bottom below the thermal insulation layer, the external gas inlet pipe is connected to the second filter crucible, and two argon gas inlet pipes are arranged, which are respectively arranged on both sides of the lower temperature measuring hole, and are both connected to the lower heater; The surfaces of the upper and lower heaters, the crystal growth crucible, and the first and second filter crucibles are all coated with tantalum carbide coatings; During the SiC PVT growth process, a certain CO partial pressure is introduced into the atmosphere, and CO is used as a transmission agent to improve the transmission efficiency of the carbon component in the SiC powder, thereby increasing the growth rate of the SiC single crystal. The principle is expressed by the following chemical formula: Si 1+X C+2XCO→(1+X)SiC+XCO2。
Citation Information
Patent Citations
A method of growing high-quality silicon carbide crystals in an oxygen-containing atmosphere
CN105734672A
Reduction of carbon inclusions in sublimation grown SiC single crystals
US20080115719A1