A sodium ion oxide positive electrode material and a preparation method thereof and a vehicle

By growing sodium ion oxides in situ on CNT and using modified CNTs, combined with sodium 2-ethanesulfonate methacrylate sodium salt, the problem of poor conductivity of the positive electrode material of sodium ion battery is solved, and a high capacity and stable battery is achieved performance.

CN118630218BActive Publication Date: 2024-12-03ZHEJIANG HUAYU NADIAN NEW ENERGY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411087447.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-03
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The electronic conductivity of existing sodium ion battery positive electrode materials is poor, resulting in complex preparation process, requiring a large number of conductive materials and dispersants, and the dispersion effect is difficult to control.

Method used

Using NaxMn2-xO2-yFy@CNT positive electrode material, a uniform distribution and sufficient distribution are formed by growing sodium ion oxides on carbon nanotubes (CNTs) in situ, combining modified CNT and sodium 2-ethanesulfonate methacrylic acid. Contact conductive network.

Benefits of technology

The preparation process is simplified, the reversible capacity and cycling performance of the battery are improved, and the electronic conductivity and stability are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118630218B_ABST
    Figure CN118630218B_ABST
Patent Text Reader

Abstract

This invention discloses a sodium-ion oxide cathode material, its preparation method, and its application in vehicles. It belongs to the field of sodium-ion battery cathode materials, specifically relating to a sodium-ion oxide cathode material comprising CNTs and layered transition metal oxides. The invention prepares the sodium-ion oxide cathode material by dispersing a conductive material in a mixed solution containing N,N-dimethylformamide, ethylene glycol, and citric acid, then adding sodium carbonate, manganese trioxide, sodium fluoride, etc., followed by ball milling, cleaning, drying, and heat treatment. The sodium-ion oxide cathode material prepared by this invention can be used in battery manufacturing, resulting in batteries with good reversible capacity and cycle performance. This battery has promising applications in electric vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sodium ion battery positive electrode materials, and in particular to a sodium ion oxide positive electrode material and a preparation method and a vehicle thereof. Background Art

[0002] Sodium-ion batteries have attracted widespread attention in recent years due to their advantages such as abundant raw materials, excellent low-temperature performance, and high safety. Layered transition metal oxides have attracted widespread attention due to their advantages such as stable crystal structure, low cost, and easy preparation. However, the electronic conductivity of layered transition metal oxide positive electrode materials is poor. When preparing positive electrode sheets, a large amount of conductive materials such as conductive carbon black (SP) and carbon nanotubes (CNT) need to be added, and additional binders and dispersants are used to make the conductive materials evenly dispersed to form a conductive network, which has certain requirements for equipment and processes.

[0003] Therefore, existing methods for improving the conductivity of the positive electrode generally have the problem of complex process conditions, mainly due to uncertain formulas of dispersants, binders, and conductive agents, cumbersome adding steps, high environmental requirements (dew point room), and difficult to control dispersion effects. Summary of the invention

[0004] In order to solve the above technical problems, the present invention specifically provides the following technical solutions:

[0005] The present invention discloses a sodium ion oxide positive electrode material, the structure of which is: Na x Mn 2-x O2- y F y @CNT positive electrode material.

[0006] Preferably, x is 1.05-1.3; or, y is 0.01-0.5.

[0007] Preferably, the sodium ion oxide positive electrode material is Na 1.2 Mn 0.8 O 1.8 F 0.2 @CNT; or, Na, Mn, O, and F are grown in situ inside CNT.

[0008] Preferably, Na 1.2 Mn 0.8 O 1.8 F 0.2 In-situ growth inside CNTs.

[0009] The present invention discloses a method for preparing a sodium ion oxide positive electrode material, comprising:

[0010] Conductive materials and metal raw materials are added to the mixed solution, and sodium ion oxide positive electrode materials, namely Nax Mn 2-x O 2-y F y @CNT positive electrode material;

[0011] The conductive material includes at least one of carbon nanotubes and modified carbon nanotubes; the metal raw materials include sodium salts and manganese compounds, the sodium salts include sodium carbonate and sodium fluoride, and the manganese compounds include manganese trioxide.

[0012] Preferably, the mixed solution contains citric acid, N,N-dimethylformamide and ethylene glycol, and the N,N-dimethylformamide and ethylene glycol in the mixed solution are mixed in a volume ratio of 1-5:1-5.

[0013] Preferably, the conductive material and the mixed solution are used in a ratio of 2-5 g: 50-100 mL.

[0014] Preferably, the conductive material and sodium carbonate are used in a mass ratio of 2-5:10-20; the conductive material and manganese trioxide are used in a mass ratio of 2-5:10-20; the conductive material and citric acid are used in a mass ratio of 2-5:10-20; the conductive material and sodium fluoride are used in a mass ratio of 2-5:30-60.

[0015] More preferably, the specific preparation steps of the sodium ion oxide positive electrode material include:

[0016] 1) N,N-dimethylformamide and ethylene glycol are mixed in a volume ratio of 1-5:1-5 to obtain a mixed solution, and then CNT is added to the mixed solution in a ratio of 2-5 g:50-100 mL, and stirred at 300-600 rpm for 30-60 min;

[0017] 2) then CNT, sodium carbonate, manganese trioxide, citric acid and sodium fluoride are added in a mass ratio of 2-5:10-20:10-20:10-20:30-60, and then ball milled at 300-600 rpm for 6-10 hours;

[0018] 3) Collect the residue by filtration, wash it with deionized water for 3-5 times, wash it with ethanol for 3-5 times, and then dry it at 60-100℃ for 3-5h.

[0019] 4) Then, heat treatment is performed under vacuum at 600-800℃ for 12-24h to prepare the sodium ion oxide positive electrode material. Too much CNT will result in too low positive electrode loading. Therefore, the amount of CNT should be within an appropriate range in the preparation of Na x Mn 2-x O 2-y F y@CNT positive electrode material Without CNT material, the electronic conductivity will be too poor and Na x Mn 2- x O 2-y F y @Performance of CNT positive electrode materials; if Na x Mn 2-x O 2-y F y Directly mixed with CNT, Na x Mn 2-x O 2-y F y It is impossible to distribute completely evenly in CNT, and Na x Mn 2-x O 2-y F y It is only in simple contact with CNT and will not be anchored on CNT. x Mn 2-x O 2-y F y @In CNT positive electrode materials, Na x Mn 2-x O 2-y F y Grown in situ within CNTs, the material is evenly distributed and is anchored and in full contact with the CNTs, which can improve the capacity and cycle performance of the battery.

[0020] In one embodiment of the present invention, a sodium ion oxide positive electrode material is prepared.

[0021] Preferably, the conductive material is a modified carbon nanotube prepared from carbon nanotubes and D-cysteine ​​hydrochloride. The modified CNT is used to prepare a sodium ion oxide positive electrode material, and then the sodium ion oxide positive electrode material is used to prepare a battery, so that the battery has good reversible capacity and cycle performance. The modified CNT may improve the Na x Mn 2-x O 2-y F y Dispersion in sodium ion oxide cathode materials, and the use of modified CNT and Na x Mn 2-x O 2-y F y It can provide better anchoring and contact, improve the electronic conductivity of the sodium ion oxide positive electrode material, thereby improving the reversible capacity of the battery and maintaining the cycle stability of the battery.

[0022] In one embodiment of the present invention, the steps of preparing the modified CNT include:

[0023] The CNTs are dispersed in the mixed acid, heated in a water bath, cooled to room temperature, and then deionized water is added. The residue is collected by filtration, washed and dried to obtain carboxylated CNTs. The carboxylated CNTs are then dispersed in SOCl 2 The mixture is then washed and filtered, and the residue is collected and dried to obtain chlorinated CNTs; D-cysteine ​​hydrochloride and the chlorinated CNTs are then dispersed in ethyl acetate, and then filtered. The residue is collected and dried to obtain modified CNTs.

[0024] Preferably, the mixed acid comprises concentrated sulfuric acid and concentrated nitric acid.

[0025] Preferably, concentrated sulfuric acid and concentrated nitric acid in the mixed acid are used in a volume ratio of 1-5:1.

[0026] Preferably, CNT and mixed acid are used in a ratio of 1-2 g: 10-20 mL.

[0027] Preferably, the mixed acid and deionized water are used in a volume ratio of 1-5:1-5.

[0028] Preferably, carboxylated CNT and SOCl 2 Use at a ratio of 2-3g:20-40mL.

[0029] Preferably, ethyl acetate and chlorinated CNT are used in a ratio of 5-10 mL: 1-2 g.

[0030] Preferably, D-cysteine ​​hydrochloride and chlorinated CNT are used in a mass ratio of 1:2-4.

[0031] More preferably, the specific preparation steps of the modified CNT include:

[0032] 1) Mix concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1-5:1 to obtain a mixed acid, then add CNT and the mixed acid in a ratio of 1-2 g: 10-20 mL to the mixed acid, ultrasonically clean for 30-60 min, heat in a water bath at 60-80° C. for 12-24 h, cool to room temperature, add the mixed acid and deionized water in a volume ratio of 1-5:1-5 to deionized water, then filter, collect the filter residue, wash the filter residue with deionized water until it is neutral, and then vacuum dry to obtain carboxylated CNT;

[0033] 2) Carboxylated CNTs and SOCl 2 Mix in a ratio of 2-3g:20-40mL, ultrasonically homogenize, and heat in an oil bath at 60-70℃ for 12-24h under nitrogen protection, then heat to remove SOCl 2 , adding tetrahydrofuran for washing, then filtering, collecting the filter residue, and vacuum drying to obtain chlorinated CNT;

[0034] 3) Ethyl acetate, D-cysteine ​​hydrochloride and chlorinated CNT are mixed in a ratio of 10-20 mL: 1 g: 2-4 g, and then ultrasonicated at 60-70° C. for 5-10 h, heated in an oil bath at 60-70° C. for 12-24 h, and then filtered to collect the residue, and vacuum dried to obtain modified CNT.

[0035] In one embodiment of the present invention, sodium methacrylate 2-ethanesulfonate is also added in the preparation of the sodium ion oxide positive electrode material.

[0036] Preferably, the specific preparation steps of the sodium ion oxide positive electrode material include:

[0037] 1) N,N-dimethylformamide and ethylene glycol are mixed in a volume ratio of 1-5:1-5 to obtain a mixed solution, and then the modified CNT is added to the mixed solution in a ratio of 2-5 g of the modified CNT to the mixed solution: 50-100 mL, and stirred at 300-600 rpm for 30-60 min;

[0038] 2) Then, sodium carbonate, manganese trioxide, citric acid, sodium fluoride and methacrylate 2-ethanesulfonate sodium salt are added in sequence with a mass ratio of 2-5:10-20:10-20:10-20:30-60:5-10 to modified CNT: sodium carbonate: manganese trioxide: citric acid: sodium fluoride: methacrylate 2-ethanesulfonate sodium salt, and then ball milled at 300-600 rpm for 6-10 hours;

[0039] 3) Collect the residue by filtration, wash it with deionized water for 3-5 times, wash it with ethanol for 3-5 times, and then dry it at 60-100℃ for 3-5h.

[0040] 4) Then, heat treatment is performed under vacuum at 600-800°C for 12-24h to prepare a sodium ion oxide positive electrode material. The sodium ion oxide positive electrode material prepared by adding sodium methacrylate 2-ethanesulfonate is then used to prepare a battery, so that the reversible capacity of the battery is further improved and the cycle performance of the battery is further improved. The addition of sodium methacrylate 2-ethanesulfonate may improve the structure of the sodium ion oxide positive electrode material and maintain its stability; and increase the electronic conductivity of the sodium ion oxide positive electrode material.

[0041] The present invention discloses an application of a sodium ion oxide positive electrode material in preparing a battery. The prepared sodium ion oxide positive electrode material is used to prepare a battery, which can greatly improve the cycle performance and reversible capacity of the battery. The battery prepared by the present invention can be applied to vehicles.

[0042] The invention discloses application of a sodium ion oxide positive electrode material in preparing a vehicle.

[0043] Compared with the prior art, the present invention uses CNT and layered transition metal oxide to prepare sodium ion oxide positive electrode materials, and the layered transition metal oxide is uniformly distributed in the conductive network formed by CNT. When the sodium ion positive electrode material is used to prepare the positive electrode sheet of the battery, there is no need to consider the more complicated formulas of dispersants, binders, and conductive agents, which simplifies the preparation steps, the process is simple, and the equipment requirements are low. At the same time, the present invention uses modified CNT to replace CNT to prepare the sodium ion oxide positive electrode material, and further adds methacrylate 2-ethanesulfonic acid sodium salt during the preparation process, which improves the structure and conductivity of the sodium ion oxide positive electrode material. When the sodium ion oxide positive electrode material is used to prepare a battery, the reversible capacity of the battery and the cycle performance of the battery are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 is the infrared spectrum of modified CNT.

[0045] Figure 2 This is a graph showing the cycle performance test results.

[0046] Figure 3 This is the AC impedance test result diagram.

[0047] Figure 4 This is the microscopic morphology of the sodium ion oxide positive electrode material. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] The experimental methods in the following examples, unless otherwise specified, are all conventional methods or conditions recommended by the manufacturer. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.

[0050] Example 1: Preparation of sodium ion oxide positive electrode material

[0051] The preparation of sodium ion oxide positive electrode material includes the following steps:

[0052] 1) Mix 30 mL of N,N-dimethylformamide (DMF) and 40 mL of ethylene glycol, add 2 g of carbon nanotubes (CNT), and stir at 400 rpm for 30 min;

[0053] 2) Continue to add 15.90g sodium carbonate, 18.95g manganese trioxide, 41.99g sodium fluoride and 15g citric acid, mix well, transfer to a ball mill, and ball mill at 400rpm for 8h;

[0054] 3) After ball milling, filter and collect the residue, wash it three times with deionized water, wash it three times with ethanol, and then dry it at 80°C for 3 hours;

[0055] 4) Heat treatment at 700℃ under vacuum for 12h to prepare the sodium ion oxide positive electrode material, namely Na 1.2 Mn 0.8 O 1.8 F 0.2 @CNT positive electrode material.

[0056] Example 2: Preparation of sodium ion oxide positive electrode material

[0057] The difference between Example 2 and Example 1 is that in Example 2, modified CNT is used instead of CNT to prepare the sodium ion oxide positive electrode material.

[0058] The preparation steps of modified CNT are as follows:

[0059] 1) Carboxylation: Concentrated sulfuric acid and concentrated nitric acid were mixed in a volume ratio of 3:1 to obtain a mixed acid; 200 mL of the mixed acid was added to 20 g of CNTs, and ultrasonically cleaned in an ultrasonic cleaner for 30 min, then heated and refluxed in a 60°C water bath for 24 h, cooled to room temperature, and then diluted with 200 mL of deionized water, and then filtered with a 0.22 μm polycarbonate membrane, the filter residue was collected, washed with deionized water until neutral, and then vacuum dried to obtain carboxylated CNTs.

[0060] 2) Acylation: Take 15g of carboxylated CNTs and add 100mL SOCl 2 After ultrasonic homogenization, under nitrogen protection, stir and reflux in a 65℃ oil bath for 24h, then increase the temperature to evaporate SOCl 2 , adding tetrahydrofuran for washing, filtering with a 0.22 μm polycarbonate membrane, collecting the filter residue and vacuum drying to obtain chlorinated CNTs.

[0061] 3) Amination: Add 5 g of D-cysteine ​​hydrochloride and 12 g of chlorinated CNTs to 60 mL of ethyl acetate, first ultrasonicate at 60 °C for 5 h, then stir and reflux in an oil bath at 60 °C for 24 h, filter with a 0.22 μm polycarbonate membrane, collect the residue and vacuum dry it to obtain modified CNTs.

[0062] Example 3: Preparation of sodium ion oxide positive electrode material

[0063] The difference between Example 3 and Example 2 is that the amount of modified CNT used in Example 3 is 5 g. The preparation of modified CNT is the same as that in Example 2.

[0064] Example 4: Preparation of sodium ion oxide positive electrode material

[0065] The difference between Example 4 and Example 3 is that in Example 4, sodium salt of 2-ethanesulfonic acid methacrylate is further added in the preparation of the sodium ion oxide positive electrode material.

[0066] The preparation of sodium ion oxide positive electrode material includes the following steps:

[0067] 1) Mix 30 mL of N,N-dimethylformamide (DMF) and 40 mL of ethylene glycol, add 5 g of modified CNT, and stir at 400 rpm for 30 min;

[0068] 2) Continue to add 15.90g sodium carbonate, 18.95g manganese trioxide, 41.99g sodium fluoride, 5g sodium methacrylate 2-ethanesulfonate and 15g citric acid, mix well, transfer to a ball mill, and ball mill at 400rpm for 8h;

[0069] 3) After ball milling, filter and collect the residue, wash it three times with deionized water, wash it three times with ethanol, and then dry it at 80°C for 3 hours;

[0070] 4) Heat treatment at 700°C under vacuum conditions for 12 hours to prepare the sodium ion oxide positive electrode material.

[0071] Example 5: Preparation of sodium ion oxide positive electrode material

[0072] The difference between Example 5 and Example 4 is that the amount of methacrylate 2-ethanesulfonate sodium salt used in Example 5 is 10 g.

[0073] Comparative Example 1: Preparation of Sodium Ion Oxide Cathode Material

[0074] The difference between Comparative Example 1 and Example 1 lies in the preparation of the sodium ion oxide positive electrode material.

[0075] The preparation of sodium ion oxide positive electrode material includes the following steps:

[0076] 1) Mix 30 mL of N,N-dimethylformamide (DMF) and 40 mL of ethylene glycol and stir at 400 rpm for 30 min;

[0077] 2) Continue to add 15.90g sodium carbonate, 18.95g manganese trioxide, 41.99g sodium fluoride and 15g citric acid, mix well, transfer to a ball mill, and ball mill at 400rpm for 8h;

[0078] 3) After ball milling, filter and collect the residue, wash it three times with deionized water, wash it three times with ethanol, and then dry it at 80°C for 3 hours;

[0079] 4) Heat treatment at 700°C under vacuum conditions for 12 hours to prepare the sodium ion oxide positive electrode material.

[0080] Comparative Example 2: Preparation of Sodium Ion Oxide Cathode Material

[0081] The difference between Comparative Example 2 and Example 2 lies in the preparation of modified CNTs.

[0082] The preparation steps of modified CNT are as follows:

[0083] 1) Carboxylation: Concentrated sulfuric acid and concentrated nitric acid were mixed in a volume ratio of 3:1 to obtain a mixed acid; 200 mL of the mixed acid was added to 20 g of CNTs, and ultrasonically cleaned in an ultrasonic cleaner for 30 min, then heated and refluxed in a 60°C water bath for 24 h, cooled to room temperature, and then diluted with 200 mL of deionized water, and then filtered with a 0.22 μm polycarbonate membrane, the filter residue was collected, washed with deionized water until neutral, and then vacuum dried to obtain carboxylated CNTs.

[0084] 2) Acylation: Take 15g of carboxylated CNTs and add 100mL SOCl 2 After ultrasonic homogenization, under nitrogen protection, stir and reflux in a 65℃ oil bath for 24h, then increase the temperature to evaporate SOCl 2 , adding tetrahydrofuran for washing, filtering with a 0.22 μm polycarbonate membrane, collecting the filter residue and vacuum drying to obtain chlorinated CNTs.

[0085] 3) Amination: Add 1 g of D-cysteine ​​hydrochloride and 12 g of chlorinated CNTs to 60 mL of ethyl acetate, first ultrasonicate at 60 °C for 5 h, then stir and reflux in an oil bath at 60 °C for 24 h, filter with a 0.22 μm polycarbonate membrane, collect the residue and vacuum dry it to obtain modified CNTs.

[0086] Experimental Example 1: Infrared spectrum of modified CNT

[0087] The infrared spectrum of the modified CNT prepared in Example 2 of the present invention is as follows: Figure 1 As shown in the figure, due to the low transmittance of CNT, only a few peaks can be seen in the infrared spectrum, at 1604cm -1 The absorption peak at 2902cm is caused by amide stretching vibration. -1 The absorption peak at is the stretching vibration peak of methyl group.

[0088] Test Example 2: First charge and discharge test

[0089] Take 1g of polyvinylidene fluoride (PVDF) and dissolve it in 24g of N-methylpyrrolidone (NMP), add 9g of sodium ion battery oxide positive electrode material, homogenize at 1000rmp for 20min, then prepare it into pole pieces and assemble button half-cells for testing.

[0090] The sodium ion oxide positive electrode materials prepared in Examples 1-5 and Comparative Example 2 were assembled into button-type half-cells according to the above steps.

[0091] The button half-cell of the sodium ion oxide positive electrode material prepared in Comparative Example 1 was prepared as follows: 1 g of polyvinylidene fluoride (PVDF) was dissolved in 24 g of N-methylpyrrolidone (NMP), 9 g of the mixture was added, and the mixture was homogenized at 1000 rpm for 20 min, and then a pole piece was prepared, and a button half-cell was assembled for testing. The mixture includes a sodium ion oxide positive electrode material and CNT, wherein the sodium ion oxide positive electrode material and CNT are mixed in a mass ratio of 3:1.

[0092] The test conditions of the button half-cell are voltage range 1.5-4V, rate 0.2C, and the results are shown in Table 1.

[0093] Table 1 First charge and discharge test results

[0094]

[0095] In the present invention, sodium carbonate, manganese trioxide, sodium fluoride and CNT are mixed in a mixed solution of DMF and ethylene glycol containing citric acid, and then ball milled, filtered and dried, and then subjected to high-temperature vacuum heat treatment to prepare a Na2O3 containing sodium, manganese, fluoride and CNT. 1.2 Mn 0.8 O 1.8 F 0.2 @CNT positive electrode material, then Na 1.2 Mn 0.8 O 1.8 F 0.2 @CNT positive electrode material is made into button battery.

[0096] Compared with Example 1, Examples 2-3 show that the use of modified CNTs in sodium ion oxide positive electrode materials can improve the reversible capacity of button batteries. By modifying CNTs, the electronic conductivity and dispersion of CNTs may be improved, thereby improving the reversible capacity of button batteries. Compared with Comparative Example 1, Example 1 shows that when preparing sodium ion oxide positive electrode materials, CNTs are used in different steps, with different effects. Through the research of the present invention, in the preparation of Na 1.2 Mn 0.8 O 1.8 F 0.2 CNTs are added to the material step to make the synthesis of Na1.2 Mn 0.8 O 1.8 F 0.2 The raw materials of the material are mixed with CNT in situ to obtain the sodium ion oxide positive electrode material, which can further improve the reversible capacity of the button battery.

[0097] Comparison between Examples 2-3 and Comparative Example 2 further indicates that the degree of modification of the modified CNT plays an important role in the preparation of the sodium ion oxide positive electrode material. The degree of modification of the modified CNT in Comparative Example 2 is relatively small, and the reversible capacity of the button battery obtained therefrom is relatively small, that is, when the amount of the modifier D-cysteine ​​hydrochloride used in the modification of the CNT is too small, the obtained sodium ion oxide positive electrode material does not have the effect of improving the reversible capacity of the button battery. Therefore, the degree of modification of the CNT needs to meet the conditions of the present invention, otherwise the effect will be poor.

[0098] Compared with Example 3, Examples 4-5 show that when the modified CNT of the present invention is used to prepare the sodium ion oxide positive electrode material, sodium methacrylate 2-ethanesulfonate can be further added. Under the action of modified CNT and other raw materials, the use of sodium methacrylate 2-ethanesulfonate can improve the reversible capacity of the button battery; sodium methacrylate 2-ethanesulfonate when used together with the above components may improve the structure of the sodium ion oxide positive electrode material, thereby improving the electronic conductivity of the sodium ion oxide positive electrode material, thereby improving the reversible capacity of the button battery.

[0099] Test Example 3: Cyclic Performance Test

[0100] According to Test Example 2, the sodium ion oxide positive electrode materials prepared in Examples 1-5 and Comparative Examples 1-2 were assembled into button-type half-cells, and 400 charge and discharge cycle tests were performed at a current of 0.2C. The capacity retention rate was used to characterize the cycle performance test of the button-type battery assembled with the sodium ion oxide positive electrode materials. The results are shown in Table 2.

[0101] Capacity retention rate calculation formula R=X 1 / X 2 , where X 1 For the first test of gram capacity, X 2 is the capacity in grams after 400 cycles.

[0102] Table 2 Cycle performance results

[0103]

[0104] In the present invention, sodium carbonate, manganese trioxide, sodium fluoride and CNT are mixed in a mixed solution of DMF and ethylene glycol containing citric acid, and then ball milled, filtered and dried, and then subjected to high-temperature vacuum heat treatment to prepare a Na2O3 containing sodium, manganese, fluoride and CNT. 1.2 Mn 0.8 O 1.8 F 0.2 @CNT positive electrode material, then Na 1.2 Mn 0.8 O 1.8 F 0.2 @CNT positive electrode material is made into button battery.

[0105] Compared with Example 1, Examples 2-3 show that the use of modified CNT in the sodium ion oxide positive electrode material has a higher capacity retention rate of the button battery; by modifying CNT, a button battery with good cycle performance is obtained. The modified CNT may improve the electronic conductivity and dispersion, thereby making the button battery have better cycle performance. Compared with Comparative Example 1, Example 1 shows that when preparing the sodium ion oxide positive electrode material, CNT is used in different steps, which has different effects. Through the research of the present invention, in the preparation of Na 1.2 Mn 0.8 O 1.8 F 0.2 CNTs are added to the material step to make the synthesis of Na 1.2 Mn 0.8 O 1.8 F 0.2 The raw materials of the material are mixed with CNT in situ to obtain the sodium ion oxide positive electrode material, which can further improve the cycle performance of the button battery.

[0106] Comparison between Examples 2-3 and Comparative Example 2 further demonstrates that the degree of modification of the modified CNT plays an important role in the preparation of the sodium ion oxide positive electrode material. The degree of modification of the modified CNT in Comparative Example 2 is relatively small, and the cycle performance of the button battery obtained therefrom is relatively poor. That is, when the amount of the modifier D-cysteine ​​hydrochloride used in the modification of the CNT is too small, the obtained sodium ion oxide positive electrode material does not have the effect of improving the cycle performance of the button battery. Therefore, the degree of modification of the CNT needs to meet the conditions of the present invention, otherwise the effect will be poor.

[0107] Comparing Example 3 with Example 4-5, it is shown that when the modified CNT of the present invention is used to prepare the sodium ion oxide positive electrode material, sodium methacrylate 2-ethanesulfonate can be further added. Under the action of modified CNT and other raw materials, the use of sodium methacrylate 2-ethanesulfonate can improve the cycle performance of the button cell; sodium methacrylate 2-ethanesulfonate, when used together with the above components, may improve the structure of the sodium ion oxide positive electrode material and maintain the stability of the structure, so that the button cell has better cycle performance.

[0108] Test Example 4: Electrochemical Performance Study

[0109] The electrochemical performance of the sodium ion oxide positive electrode materials prepared in Example 1 and Comparative Example 1 was further studied. The sodium ion oxide positive electrode materials prepared in Example 1 and Comparative Example 1 were assembled into button-type half-cells according to the steps in Experimental Example 2 for testing.

[0110] 1. Cyclic performance test of button half-cell

[0111] The test conditions of button half-cell are voltage range 1.5-4V, rate 0.2C, the results are as follows Figure 2 As shown in the figure, from the initial capacity, the first discharge capacity of the button half-cell prepared in Example 1 is 135 mAh g -1 , while the first discharge capacity of the button-type half-cell prepared in Comparative Example 1 is only 130 mAh g -1 After 400 cycles, the capacity retention rate of the button-type half-battery prepared in Example 1 is 95.9%, while the capacity retention rate of the button-type half-battery prepared in Comparative Example 1 is only 84.6%.

[0112] The above results show that the button-type half-cell prepared by the sodium ion oxide positive electrode material in Example 1 has good cycle performance and high battery capacity.

[0113] 2. AC impedance test of button half-cell

[0114] The disturbance voltage amplitude applied during the test was 5mV, and the frequency range was 0.01-100000Hz. The results are as follows Figure 3 As shown, it can be seen that the button-type half-cells prepared in Example 1 and Comparative Example 1 both have the characteristics of a high-frequency semicircular arc and a low-frequency oblique line, which correspond to the interfacial electrochemical reaction impedance and diffusion impedance of the battery, respectively. The electrochemical impedance of the button-type half-cell prepared in Example 1 is less than that of the button-type half-cell prepared in Comparative Example 1, indicating that the sodium ion oxide positive electrode material in Example 1 has good electronic conductivity.

[0115] Test Example 5: Microscopic morphology of sodium ion oxide positive electrode material

[0116] The sodium ion oxide positive electrode material of Example 1 was tested by scanning electron microscope, and the results are as follows: Figure 4 As shown in the figure, it can be seen that Na, Mn, O, and F are in-situ grown inside the CNTs, the materials are evenly distributed, and the CNTs are anchored and in full contact.

[0117] The embodiments and / or implementation methods described above are only used to illustrate the preferred embodiments and / or implementation methods for realizing the technology of the present invention, and are not intended to impose any form of limitation on the implementation methods of the technology of the present invention. Any technical personnel in this field may make slight changes or modifications to other equivalent embodiments without departing from the scope of the technical means disclosed in the content of the present invention, but they should still be regarded as technologies or embodiments that are essentially the same as the present invention.

Claims

1. A method for preparing a sodium ion oxide positive electrode material, comprising: 1) N,N-dimethylformamide and ethylene glycol are mixed in a volume ratio of 1-5:1-5 to obtain a mixed solution, and then the modified CNT is added to the mixed solution in a ratio of 2-5 g of the modified CNT to the mixed solution: 50-100 mL, and stirred at 300-600 rpm for 30-60 min; 2) Then, sodium carbonate, manganese trioxide, citric acid, sodium fluoride and methacrylate 2-ethanesulfonate sodium salt are added in sequence with a mass ratio of 2-5:10-20:10-20:10-20:30-60:5-10 to modified CNT: sodium carbonate: manganese trioxide: citric acid: sodium fluoride: methacrylate 2-ethanesulfonate sodium salt, and then ball milled at 300-600 rpm for 6-10 hours; 3) Filter and collect the residue, wash it with deionized water for 3-5 times, wash it with ethanol for 3-5 times, and then dry it at 60-100℃ for 3-5h; 4) Then, heat treatment was performed under vacuum at 600-800°C for 12-24h to prepare a sodium ion oxide positive electrode material; namely, Na x Mn 2-x O 2-y F y @CNT positive electrode material; Na x Mn 2-x O 2-y F y @CNT positive electrode material is Na 1.2 Mn 0.8 O 1.8 F 0.2 @CNT positive electrode material; Preparation of modified carbon nanotubes: CNTs are dispersed in a mixed acid, heated in a water bath, cooled to room temperature, and then deionized water is added, and the residue is filtered and collected, washed and dried to obtain carboxylated CNTs; then the carboxylated CNTs are dispersed in SOCl2, oil bathed, and then washed, filtered, the residue is collected and dried to obtain chlorinated CNTs; then D-cysteine ​​hydrochloride and chlorinated CNTs are dispersed in ethyl acetate, oil bathed, and then filtered, the residue is collected and dried to obtain modified CNTs; the mixed acid includes concentrated sulfuric acid and concentrated nitric acid, and the concentrated sulfuric acid and concentrated nitric acid in the mixed acid are The volume ratio is 1-5:1, CNT and mixed acid are used in a ratio of 1-2g:10-20mL; mixed acid and deionized water are used in a volume ratio of 1-5:1-5; carboxylated CNT and SOCl2 are used in a ratio of 2-3g:20-40mL; ethyl acetate and chlorinated CNT are used in a ratio of 5-10mL:1-2g; D-cysteine ​​hydrochloride and chlorinated CNT are used in a mass ratio of 1:2-4; the modified carbon nanotubes and the mixed solution are used in a ratio of 2-5g:50-100mL; The modified carbon nanotubes and sodium carbonate are used in a mass ratio of 2-5:10-20; the modified carbon nanotubes and manganese trioxide are used in a mass ratio of 2-5:10-20; the modified carbon nanotubes and sodium fluoride are used in a mass ratio of 2-5:30-60.

2. The preparation method according to claim 1, characterized in that: The mixed solution contains citric acid, N,N-dimethylformamide and ethylene glycol, and the N,N-dimethylformamide and ethylene glycol in the mixed solution are mixed in a volume ratio of 1-5:1-5.

3. The preparation method according to claim 1, characterized in that: The modified carbon nanotubes and citric acid are used in a mass ratio of 2-5:10-20.

4. The sodium ion oxide positive electrode material prepared by the method according to any one of claims 1 to 3, wherein the structure is: Na x Mn 2- x O 2-y F y @CNT positive electrode material, characterized by: The sodium ion oxide positive electrode material is Na 1.2 Mn 0.8 O 1.8 F 0.2 @CNT; Na 1.2 Mn 0.8 O 1.8 F 0.2 The in-situ growth is inside the CNT, and the CNT is the modified carbon nanotube as described in claim 1.

5. Use of the sodium ion oxide positive electrode material according to claim 4 in preparing a battery.

Citation Information

Patent Citations

  • Sodium manganate material applied to high-power sodium battery and preparation method of sodium manganate material

    CN116443938A

  • Preparation and application method of fluorine-doped zinc-manganese-based layered oxide positive electrode material

    CN117594782A

  • Sodium-ion battery positive electrode material, preparation method therefor and use thereof

    WO2022160534A1