Welding method and welding equipment
By setting a metal ring on the composite frame, we avoid contact with the shaft shoulder of the welding tool, combined with narrow margin large shaft shoulder and deviation welding technology, the problems of welding tool damage and insufficient material heat generation in friction stir welding are solved, and the composite board is improved Welding strength and welding quality.
Patent Information
- Application Number
- CN202411049826.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-01
AI Technical Summary
During friction stir welding, the thickness of the aluminum alloy is too small, and the shoulders of the welding tool are prone to contact with hard metal, resulting in damage to the welding tool or insufficient heat generation of the material, which in turn causes welding defects and causes low welding joint strength.
By setting a metal ring on the composite frame, the welding tool shoulders are prevented from directly contacting the first metal layer, and friction stir welding is used for narrow margin large shoulders, and the welding tool is controlled to deviate along the main welding interface from the secondary welding interface during the welding process. Improve connection area and welding strength.
It effectively avoids the wear of the shoulder of the welding tool, reduces the thickness of the second metal layer, realizes high-strength connection, and improves the welding strength and welding quality of the composite board.
Smart Images

Figure CN118635654B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of friction stir welding, and in particular to a welding method and a welding device. Background Art
[0002] Composite plates such as aluminum-titanium composite plates, aluminum-steel composite plates or aluminum-copper composite plates have the advantages of corrosion resistance, light weight, high strength, long service life and economy, and are widely used. Due to the manufacturing process, the thickness of such composite plates is limited. In order to increase the thickness of the composite plates, aluminum plates can be welded on the aluminum alloy side of the composite plates. Generally, in order to reduce costs, it is necessary to reduce the thickness of the aluminum alloy in the composite plate as much as possible. However, if the thickness of the aluminum alloy is too small, during the friction stir welding process between the aluminum alloy and the aluminum plate, the shoulder of the stirring head is easy to contact the hard metal in the composite plate (such as the titanium alloy of the titanium-aluminum composite plate), causing damage to the welding tool. If the welding tool uses a small shoulder to avoid contact between the shoulder and the hard metal, it is easy to cause insufficient heat generation of the material, which is easy to cause welding defects and result in low weld connection strength. Summary of the invention
[0003] Embodiments of the present application provide a welding method and a welding device.
[0004] The welding method of the embodiment of the present application is used to form a composite plate, and the welding method includes:
[0005] Obtain a composite frame, a metal back plate and a metal ring, wherein the composite frame includes a first metal layer and a second metal layer;
[0006] Placing the composite frame and the metal back plate on a welding table, wherein the metal back plate is adjacent to the second metal layer;
[0007] The metal ring cover is arranged on the composite frame;
[0008] The metal ring, the second metal layer and the metal back plate are subjected to stir friction welding by the welding tool to form the composite plate.
[0009] In some embodiments, the metal ring includes multiple pieces, and the step of covering the metal ring on the composite frame includes:
[0010] A plurality of metal rings are respectively covered on two opposite sides of the composite frame.
[0011] In some embodiments, the step of welding the metal ring, the second metal layer, and the metal back plate by the welding tool to form the composite plate comprises:
[0012] Performing friction stir welding on the metal ring, the second metal layer and the metal back plate by using the welding tool with a single-sided friction stir welding process to form the composite plate; or
[0013] The metal ring, the second metal layer and the metal back plate are subjected to friction stir welding by using the welding tool with a double-sided friction stir welding process to form the composite plate.
[0014] In some embodiments, the metal ring, the second metal layer and the metal back plate are subjected to friction stir welding by the welding tool to form the composite plate, comprising:
[0015] At least one splicing interface is used as a main welding interface, and the splicing interface connected to the main welding surface and located on the side of the main welding interface is used as a secondary welding interface;
[0016] The welding tool is controlled to weld along the main welding interface and at least partially deviate from the main welding interface to weld toward the secondary welding interface, so as to form the composite plate.
[0017] In some embodiments, the portion of the welding tool welded along the main welding interface forms a stable path, and the portion of the welding tool that deviates from the main welding interface and is welded toward the secondary welding interface forms a deviated path, and the deviated path includes an arc path, an annular path, or a combination of one or more of the arc path, the annular path, and a straight path.
[0018] In some embodiments, the speed at which the welding tool moves along the main welding interface is a first speed, and the speed at which the welding tool moves away from the main welding interface is a second speed, and the second speed is less than the first speed.
[0019] In some embodiments, the rotation speed of the welding tool when moving along the main welding interface is a first rotation speed, and the rotation speed of the welding tool when moving away from the main welding interface is a second rotation speed, and the second rotation speed is greater than the first rotation speed.
[0020] In certain embodiments, the deviation path is an arc path, and the maximum distance that the center of the welding tool deviates from the main welding interface does not exceed the radius of the root of the stirring needle of the welding tool.
[0021] In some embodiments, the welding method further comprises:
[0022] When the welding tool performs friction stir welding on the metal ring, the second metal layer and the metal back plate, heating and / or emitting ultrasonic waves are performed on the friction stir welding area.
[0023] In some embodiments, the welding tool is of the type of dynamic shoulder / static shoulder.
[0024] In certain embodiments, the thickness of the second metal layer is less than the radius of the shoulder of the welding tool.
[0025] In certain embodiments, the metal ring is flush with the metal backing plate.
[0026] In certain embodiments, the height of the metal ring is 0.1-80 mm.
[0027] In some embodiments, the first distance between the inner wall of the metal ring and the inner wall of the composite frame ranges from 0 to 100 mm.
[0028] In some embodiments, the second distance between the outer wall of the metal ring and the outer wall of the composite frame ranges from 0 to 90 mm.
[0029] The welding equipment of the embodiment of the present application is used to form a composite plate, and the welding equipment includes:
[0030] An acquisition module, used for acquiring a composite frame, a metal back plate and a metal ring, wherein the composite frame includes a first metal layer and a second metal layer;
[0031] A mounting module, used for placing the composite frame and the metal back plate on a welding table, wherein the metal back plate is adjacent to the second metal layer;
[0032] A fixing module, used for fixing the metal ring cover on the composite frame;
[0033] The control module is used to stir friction welding the metal ring, the second metal layer and the metal back plate by using a welding tool to form the composite plate.
[0034] In the welding method and welding equipment of the implementation mode of the present application, by setting the metal ring cover on the composite frame, when the welding tool performs stir friction welding on the metal ring, the metal back plate and the second metal layer, the metal ring can prevent the shoulder of the welding tool from directly contacting the first metal layer of the metal ring, thereby avoiding the first metal layer from wearing the shoulder of the welding tool, and the thickness of the second metal layer can be reduced, realizing narrow margin and large shoulder stir friction welding and saving costs. In addition, the setting of the metal ring enables the metal ring, the metal back plate and the composite frame to be butt-jointed during stir friction welding, thereby increasing the connection area, thereby realizing high-strength connection, and improving the strength of the composite plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0036] Figure 1 It is one of the flow diagrams of the welding method of certain embodiments of the present application;
[0037] Figure 2 is a schematic diagram of a module of a welding device according to some embodiments of the present application;
[0038] Figure 3 It is a schematic diagram of the positions of the composite frame and the metal back plate of certain embodiments of the present application;
[0039] Figure 4 This is a schematic diagram of a scene in which a metal ring is covered on a composite frame in certain embodiments of the present application;
[0040] Figure 5 is a schematic diagram of a welding process according to some embodiments of the present application;
[0041] Figure 6 This is the second schematic flow diagram of the welding method of certain embodiments of the present application;
[0042] Figure 7 This is the third schematic flow diagram of the welding method of certain embodiments of the present application;
[0043] Figure 8 It is a schematic diagram of a single-sided welding scenario in certain embodiments of the present application;
[0044] Fig. 9 This is one of the schematic diagrams of double-sided welding scenarios in certain embodiments of the present application;
[0045] Fig.10 This is the second schematic diagram of a double-sided welding scenario in certain embodiments of the present application;
[0046] Fig.11 This is a fourth schematic flow diagram of a welding method according to certain embodiments of the present application;
[0047] Fig.12 It is one of the scene schematic diagrams of the welding process of certain embodiments of the present application;
[0048] Fig.13 This is the second schematic diagram of a welding process in some embodiments of the present application;
[0049] Fig.14 This is the third schematic diagram of a welding process in some embodiments of the present application;
[0050] Fig.15 This is the fifth flow chart of the welding method of certain embodiments of the present application.
[0051] Description of the main figures
[0052] Composite frame 1, first metal layer 11, second metal layer 12, metal back plate 2, metal ring 3;
[0053] Welding tool 20, stirring needle 21, shaft shoulder 22;
[0054] Splicing interface 30, primary welding interface 31, secondary welding interface 32;
[0055] Welding path 40, stable path 41, deviation path 42;
[0056] Welding equipment 100 , acquisition module 110 , installation module 120 , fixing module 130 , control module 140 , and auxiliary module 150 . DETAILED DESCRIPTION
[0057] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar elements or elements having the same or similar functions from beginning to end. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the embodiments of the present invention, and cannot be understood as limiting the embodiments of the present invention.
[0058] See also Figure 1 as well as Figure 3-5 , the embodiment of the present application provides a welding method for forming a composite plate, the welding method comprising:
[0059] 01: Get a composite frame 1, a metal back plate 2 and a metal ring 3, where the composite frame 1 includes a first metal layer 11 and a second metal layer 12;
[0060] 02: The composite frame 1 and the metal back plate 2 are placed on a welding table, and the metal back plate 2 is adjacent to the second metal layer 12;
[0061] 03: Cover the metal ring 3 on the composite frame 1;
[0062] 04: The metal ring 3, the second metal layer 12 and the metal back plate 2 are subjected to friction stir welding by a welding tool 20 to form a composite plate.
[0063] See also Figure 2 This embodiment further provides a welding device 100 , which is used to form a composite plate. The welding device 100 includes an acquisition module 110 , a mounting module 120 , a fixing module 130 and a control module 140 .
[0064] Step 01 can be implemented by the acquisition module 110, step 02 can be implemented by the installation module 120, step 03 can be implemented by the fixing module 130, and step 04 can be implemented by the control module 140. That is to say, the acquisition module 110 is used to acquire the composite frame 1, the metal back plate 2 and the metal ring 3, and the composite frame 1 includes a first metal layer 11 and a second metal layer 12. The installation module 120 is used to set the composite frame 1 and the metal back plate 2 on the welding table, and the metal back plate 2 is adjacent to the second metal layer 12; the fixing module 130 is used to cover the metal ring 3 on the composite frame 1; the control module 140 is used to stir friction welding the metal ring 3, the second metal layer 12 and the metal back plate 2 through the welding tool 20 to form a composite plate.
[0065] In the welding method and welding equipment 100 of the present application, by covering the metal ring 3 on the composite frame 1, when the welding tool 20 performs stir friction welding on the metal ring 3, the metal back plate 2 and the second metal layer 12, the metal ring 3 can prevent the shoulder 22 of the welding tool 20 from directly contacting the first metal layer 11 of the metal ring 3, thereby preventing the first metal layer 11 from wearing the shoulder 22 of the welding tool 20, and the thickness of the second metal layer 12 can be reduced to achieve narrow margin and large shoulder stir friction welding and save costs. In addition, the setting of the metal ring 3 enables the metal ring 3, the metal back plate 2 and the composite frame 1 to be butt-jointed during stir friction welding, thereby increasing the connection area, thereby achieving high-strength connection, and improving the strength of the composite plate.
[0066] Please combine Figure 3-5 Specifically, the first metal layer 11 and the second metal layer 12 can both be metal alloys, and the hardness of the first metal layer 11 is greater than the hardness of the second metal layer 12, and the second metal layer 12 is used to achieve welding with the metal back plate 2. The first metal layer 11 can be a titanium alloy, a copper alloy, stainless steel, etc., and the second metal layer 12 can be an aluminum alloy, a magnesium alloy, etc. The specific materials of the first metal layer 11 and the second metal layer 12 are not limited. In this embodiment, the first metal layer 11 can be a titanium alloy and the second metal layer 12 can be an aluminum alloy.
[0067] The composite frame 1 is square, and the composite frame 1 can be formed by bending a metal composite plate including a first metal layer 11 and a second metal layer 12, or can be formed by splicing two or more metal composite plates including a first metal layer 11 and a second metal layer 12. The first metal layer 11 of the composite frame 1 constitutes the outer wall of the composite frame 1, and the second metal layer 12 constitutes the inner wall of the composite frame 1.
[0068] The metal back plate 2 and the metal ring 3 are made of the same or approximately the same material as the second metal layer 12. For example, if the second metal layer 12 is an aluminum alloy, the metal back plate 2 can be an aluminum plate, and the metal ring 3 can be made of aluminum or an aluminum alloy. In this way, the second metal layer 12, the metal back plate 2, and the metal ring 3 can be stir-friction welded by the welding tool 20 to form a composite plate together.
[0069] The metal ring 3 has a substantially identical shape to the composite frame 1, and the metal ring 3 may be formed by bending a metal plate, or by splicing two or more metal plates. The metal back plate 2 has a substantially identical shape to the second metal layer 12, and the metal back plate 2 may be formed by a single metal back plate 2, or by splicing two or more metal back plates 2.
[0070] Before performing stir friction welding, the composite frame 1 and the metal back plate 2 can be placed on a welding table. The welding table may include a clamping mechanism, and the welding table can clamp the first metal layer 11 of the composite frame 1 through the clamping mechanism. For example, the welding table may include four clamping mechanisms, and the four clamping mechanisms can respectively clamp the four outer walls of the composite frame 1. The metal back plate 2 is located inside the composite frame 1 and is adjacent to the second metal layer 12.
[0071] The height of the metal back plate 2 is greater than or equal to the height of the composite frame 1. The height difference between the metal back plate 2 and the composite frame 1 can range from 0 to 120 mm. For example, the height difference between the metal back plate 2 and the composite frame 1 can range from 0 mm, 1 mm, 2 mm, 10 mm, 20 mm, 30 mm, 50 mm, 80 mm, 100 mm, etc.
[0072] After the composite frame 1 is clamped by the welding table, the metal ring 3 can be covered on the composite frame 1 to cover the first metal layer 11 and the second metal layer 12 .
[0073] Further, the height of the metal ring 3 can range from 0.1 to 80 mm, for example, the height of the metal ring 3 can be 0.1 mm, 1 mm, 2 mm, 5 mm, 10 mm, 20 mm, 30 mm, 50 mm, 80 mm, etc. The first distance between the inner wall of the metal ring 3 and the inner wall of the composite frame 1 ranges from 0 to 100 mm, for example, the distance from the inner wall of the metal ring 3 to the inner wall of the composite frame 1 can be 0 mm, 1 mm, 10 mm, 15 mm, 20 mm, 30 mm, 50 mm or 80 mm, etc. The second distance range between the outer wall of the metal ring 3 and the outer wall of the composite frame 1 is 0-90 mm. For example, the distance from the outer wall of the metal ring 3 to the outer wall of the composite frame 1 can be 0 mm, 1 mm, 10 mm, 15 mm, 20 mm, 30 mm, 50 mm or 90 mm, etc. It can be understood that it is only necessary to ensure that the shoulder 22 of the welding tool 20 can avoid friction with the first metal layer 11 during stir friction welding, and the specific distance from the outer wall of the metal ring 3 to the outer wall of the composite frame 1 is not limited.
[0074] In some embodiments, when the metal back plate 2 is located inside the composite frame 1, the metal back plate 2 can partially protrude from the composite frame 1, so that when the metal ring 3 is covered on the composite frame 1, the metal ring 3 can be flush with the metal back plate 2. In this way, when stir friction welding is subsequently performed by the welding tool 20, the welding position is not suspended, thereby improving the welding quality.
[0075] The welding tool 20 may include a stirring pin 21 and a shoulder 22, the stirring pin 21 extends from the shoulder 22, and during the process of the welding tool 20 performing stir friction welding on the metal ring 3, the second metal layer 12 and the metal back plate 2, the welding tool 20 rotates and extends into the metal ring 3, the second metal layer 12 and the metal back plate 2 through the stirring pin 21 to stir and rub, so that the metal ring 3, the second metal layer 12 and the metal back plate 2 reach a thermoplastic state, and then the metal ring 3, the second metal layer 12 and the metal back plate 2 can be welded together. Furthermore, the metal ring 3 can be partially removed by a milling process to form a composite plate containing only the composite frame 1 and the metal back plate 2.
[0076] In some embodiments, the type of the welding tool 20 can be a static shoulder. That is, during the friction stir welding process, the main heat generation method comes from the friction between the internal stirring needle 21 and the material, and the static shoulder 22 does not rotate during the welding process, but only moves along the welding direction. The setting of the static shoulder 22 reduces the surface heat input of the welding tool 20, and the heat in the thickness direction of the workpiece is uniform, making the welding quality more stable. Secondly, the friction heat is evenly distributed, the joint structure is uniform, the weld surface is smooth, and the amount of flash is small, which can effectively inhibit the extrusion of the weld material, reduce the thinning of the weld, and reduce the probability of defects such as holes and tunnels.
[0077] In some embodiments, the type of the welding tool 20 can be a dynamic shoulder. During the friction stir welding process, the shoulder 22 and the stirring needle 21 both rotate and move in the welding direction. The rotating shoulder 22 contacts the metal back plate 2 and the metal ring 3 to participate in the friction stir. The stirring needle 21 is inserted into the weld under the cover of the shoulder 22 to stir and squeeze the plastic material, thereby achieving the connection of the materials. It can be understood that the rotation of the dynamic shoulder helps to transfer heat and pressure more evenly, improves the welding quality and efficiency, and the welding tool 20 using the dynamic shoulder has a wide range of applications and can adapt to welds with narrow welding spaces.
[0078] In some embodiments, when the shoulder 22 is a dynamic shoulder, the radius of the shoulder 22 is greater than the thickness of the second metal layer 12. That is, the coverage area of the shoulder 22 can be greater than the second metal layer 12, so that the shoulder 22 is more conducive to more uniform transfer of heat and pressure, thereby further improving the welding quality of the composite plate.
[0079] See also Figure 6 In some embodiments, the metal ring 3 includes multiple pieces, and step 03 includes:
[0080] 031, a plurality of metal rings 3 are respectively covered on two opposite sides of the composite frame 1.
[0081] Please refer to further Figure 2 In some embodiments, step 031 can be implemented by the fixing module 130 , or in other words, the fixing module 130 can be used to cover the plurality of metal rings 3 on two opposite sides of the composite frame 1 .
[0082] See also Figure 8-10 Specifically, during the welding process, the metal ring 3 may be provided on only one side of the composite frame 1, or may be provided on two opposite sides of the composite frame 1. It can be understood that due to the provision of the metal ring 3, the metal back plate 2 and the composite frame 1 are butted during the friction stir welding, the connection area is increased, and a high-strength connection is achieved. Therefore, compared with only one side being provided with the metal ring 3, the composite frame 1 having both sides provided with the metal ring 3 can further improve the welding quality of the composite plate.
[0083] See also Figure 7-10 In some embodiments, step 04 includes:
[0084] 041, using a single-sided friction stir welding process to stir friction weld the metal ring 3, the second metal layer 12 and the metal back plate 2 by using a welding tool 20 to form a composite plate; or
[0085] 042, the metal ring 3, the second metal layer 12 and the metal back plate 2 are subjected to friction stir welding by a double-sided friction stir welding process using a welding tool 20 to form a composite plate.
[0086] In some embodiments, steps 041 and 042 can be implemented by the control module 140, or in other words, the control module 140 can use the welding tool 20 to perform friction stir welding on the metal ring 3, the second metal layer 12 and the metal back plate 2 using a single-sided friction stir welding process to form a composite plate, or use the welding tool 20 to perform friction stir welding on the metal ring 3, the second metal layer 12 and the metal back plate 2 using a double-sided friction stir welding process to form a composite plate.
[0087] It should be noted that the single-sided friction stir welding process refers to single-sided welding. Compared with double-sided welding, it improves welding efficiency and reduces welding costs.
[0088] Double-sided friction stir welding is a technology that performs friction stir welding on the upper and lower sides of the plate to be welded. The double-sided friction stir welding process can effectively solve the problems existing in thick plate welding, such as uneven performance of the welding joint and easy defects.
[0089] Double-sided friction stir welding can be achieved by either single-axis drive step-by-step welding or double-axis drive welding. Single-axis drive step-by-step welding is to first complete the welding on one side of the plate to be welded, and then flip the workpiece to perform the second pass welding on the opposite side, while double-axis drive welding can weld both sides of the plate to be welded at the same time. In this embodiment, double-axis drive welding can be used. It can be understood that since welding is performed on both sides of the plate at the same time, the composite plate can be made more uniform in the thickness direction, thereby improving the overall performance of the composite plate.
[0090] See also Figure 11-14 In some embodiments, step 04 further includes:
[0091] 043, at least one splicing interface 30 is used as a main welding interface 31, and the splicing interface 30 located on the side of the main welding interface 31 is used as a secondary welding interface 32;
[0092] 044, control the welding tool 20 to weld along the main welding interface 31 and at least partially deviate from the main welding interface 31 to weld toward the secondary welding interface 32 to form a composite plate.
[0093] In some embodiments, steps 043 and 044 can be implemented by the control module 140, or in other words, the control module 140 can also be used to use at least one splicing interface 30 as a main welding interface 31, and the splicing interface 30 located on the side of the main welding interface 31 as a secondary welding interface 32, and control the welding tool 20 to weld along the main welding interface 31 and at least partially deviate from the main welding interface 31 to offset the welding to the secondary welding interface 32 to form a composite plate.
[0094] It should be noted that the splicing interface 30 can be a splicing interface 30 formed between the metal back plate 2 and the metal ring 3, a splicing interface 30 formed between the metal frame and the metal ring 3, a splicing interface 30 formed between the metal back plates 2 and the metal back plates 2 (that is, a large metal back plate 2 is formed by splicing multiple metal back plates 2), and a splicing interface 30 in the metal ring 3 (for example, the metal ring 3 is formed by splicing multiple metal plates, then a splicing interface 30 is formed between every two adjacent metal plates).
[0095] The splicing interface 30 can be divided into a butt joint interface and an overlapped interface, wherein the overlapped interface extends along the horizontal plane and the butt joint interface extends along the vertical plane. For example, the splicing interface 30 formed between the metal back plate 2 and the metal ring 3 is a butt joint interface, and the splicing interface 30 formed between the metal frame and the metal ring 3 is an overlapped interface. In this embodiment, at least one butt joint interface is used as the main welding interface 31, and the overlapped interface and the butt joint interface connected to the main welding interface 31 and located on one side or both sides of the main welding interface 31 are used as the secondary welding interface 32.
[0096] In the related art, when multiple splicing interfaces 30 are overlapping interfaces and butt interfaces, during the welding process, due to the stirring action of the stirring needle 21, the material at the overlapping interface will migrate upward along the axial direction of the stirring needle 21 under the stirring and extrusion action of the stirring needle 21, forming a hook-shaped defect. The occurrence of this defect will reduce the effective plate thickness of the material around the weld. Usually, the hook-shaped defect is formed on the forward side of the weld; at the same time, the effective connection width of the overlapping interface is small, forming a cold overlapping defect.
[0097] When the multiple joint interfaces 30 are three-joint joint interfaces and multiple-joint joint interfaces, under the action of the stirring needle 21 during welding, in the horizontal direction, the secondary welding interface 32 will migrate along the rotation direction of the stirring needle 21, forming weak connection defects such as cracks inside the weld. In the axial direction of the stirring needle 21, the material flows along the side of the stirring needle 21, and the material in the vicinity of the overlapping interface will flow upward or downward, forming a weak connection or hook-shaped defect.
[0098] Therefore, in the present embodiment, the welding tool 20 is controlled to weld along the main welding interface 31 and at least partially deviate from the main welding interface 31 to the secondary welding interface 32 for offset welding, so that the volume of the material stirred by the stirring needle 21 of the welding tool 20 at the junction of the main welding interface 31 and the secondary welding interface 32 can be increased. Compared with the welding effect of a straight weld, after the welding path 40 of the welding tool 20 is offset, the material stirring at the junction of the main welding interface 31 and the secondary welding interface 32 is more intense, and the stirring area is larger, which is beneficial to increase the effective connection width of the secondary welding interface 32, thereby reducing weak connections and cold lap defects at the junction, and improving the connection effect between multiple splicing interfaces 30, thereby ensuring the microstructure and mechanical properties of the formed weld, and improving the connection strength of the composite plate.
[0099] In some embodiments, the portion of the welding tool 20 welded along the main welding interface 31 forms a stable path 41, and the portion of the welding tool 20 welded offset from the main welding interface 31 to the secondary welding interface 32 forms a deviated path 42, and the deviated path 42 includes an arc path, an annular path, or a combination of one or more of an arc path, an annular path, and a straight path.
[0100] Please refer to further Fig.12 or Fig.14 According to some embodiments of the present invention, the deviation path 42 can be an arc path to increase the volume of the material stirred by the stirring needle 21 of the welding tool 20 at the portion where the secondary welding interface 32 is connected to the main welding interface 31, thereby facilitating increasing the effective welding connection width of the secondary welding interface 32.
[0101] Please refer to further Fig.13 In some embodiments, the deviation path 42 can be a combination of multiple connected ones of an arc path, an annular path, and a straight path. Exemplarily, the deviation path 42 includes an annular path and two arc paths, one end of the two arc paths is respectively connected to the starting end and the end of the annular path, and the other ends of the two arc paths are connected to the stable path 41. The two arc paths and the partial annular path are located on one side of the stable path 41, and the other partial annular path is located on the other side of the stable path 41.
[0102] Please refer to further Fig.14 According to some embodiments of the present invention, the deviation path 42 may be an annular path, the starting end and the end of the annular path coincide, and the starting end and the end of the annular path are both connected to the stable path 41. The annular path may be a circular annular path, a rectangular path, or a rounded rectangular path. The annular path is a rounded rectangular path, the annular path is located on one side of the stable path 41, and the starting end and the end of the annular path are respectively connected to the stable path 41.
[0103] In the embodiment of the present invention, the deviation path 42 includes an annular path, or a combination of multiple connected arc paths, annular paths and straight paths. In this way, the material of the portion where the secondary welding interface 32 is connected to the main welding interface 31 will be stirred multiple times during the movement of the welding tool 20 along the deviation path 42, and the multiple stirring directions may be the same or different.
[0104] The rotation direction of the stirring needle 21 of the welding tool 20 is clockwise, and the moving direction of the stirring needle 21 when moving along the main welding interface 31 is from top to bottom in the figure. Since when the welding tool 20 moves along the annular path, the moving direction of the welding tool 20 when moving in the part where the annular path overlaps with the stable path 41 is opposite to the moving direction when moving in the part of the annular path away from the stable path 41. Therefore, the stirring direction of the material at the secondary welding interface 32 located in the annular path by the welding tool 20 is also opposite, that is, the material flow direction is also opposite. For example, the material first rotates along the first direction to form a hook-shaped defect, and then the material rotates along the second direction. The first direction and the second direction are opposite. At this time, the material of the hook-shaped defect part can be re-screwed into the interior of the workpiece to be welded, which is beneficial to eliminate the hook-shaped defect.
[0105] At the same time, the material can also flow in the same direction for multiple times, thereby increasing the stirring degree at the junction of the secondary welding interface 32 and the main welding interface 31 and increasing the effective connection width of the secondary welding interface 32; and the cracks formed by the migration of the secondary welding interface 32 during the first stirring can also be broken under the multiple stirring actions of the welding tool 20, thereby increasing the material mixing degree at the junction of the main welding interface 31 and the secondary welding interface 32, thereby improving the microstructure and mechanical properties of the weld area.
[0106] In some embodiments, the rotation speed of the welding tool 20 when moving along the main welding interface 31 is in the range of 50-50000 rpm, the movement speed is in the range of 5-100000 mm / min, and the dwell time is in the range of 0-50 seconds. It is understood that the rotation speed, movement speed and dwell time of the welding tool 20 can be adjusted according to actual conditions, so the specific values are not limited.
[0107] In some embodiments, the speed of the welding tool 20 moving along the main welding interface 31 is a first speed, and the speed of the welding tool 20 moving away from the main welding interface 31 is a second speed, and the second speed is less than the first speed.
[0108] The welding path 40 of the welding tool 20 includes a stable path 41 and a deviated path 42. The portion of the welding path 40 of the welding tool 20 along the main welding interface 31 is formed as the stable path 41, and the portion of the welding path 40 of the welding tool 20 deviating from the main welding interface 31 is formed as the deviated path 42. That is to say, the speed of the welding tool 20 moving along the deviated path 42 is slow, which can increase the number of stirring times of the material at the junction of the main welding interface 31 and the secondary welding interface 32, so that the material stirring at this location is more intense, which is beneficial to increase the uniformity of the material at this location, thereby improving the welding connection effect, reducing the generation of defects, and further ensuring the microstructure and mechanical properties of the weld.
[0109] According to some embodiments of the present invention, the ratio of the second speed to the first speed is α, 0.2<α<1. For example, the ratio of the second speed to the first speed is 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or any value between any adjacent values therein, etc.
[0110] The ratio of the second speed to the first speed is within this range. On the one hand, the second speed will not be too small, and will not increase the welding time too much, or cause plastic deformation of the material around the junction of the main welding interface 31 and the secondary welding interface 32; on the other hand, the number of stirring times for the material at the junction of the main welding interface 31 and the secondary welding interface 32 can be increased, so that the material at this junction is stirred more violently, which is beneficial to increase the uniformity of the material at this junction, thereby improving the welding connection effect, reducing the generation of defects, and further ensuring the microstructure and mechanical properties of the weld.
[0111] The rotation speed of the welding tool 20 when moving along the main welding interface 31 is the first rotation speed, and the rotation speed of the welding tool 20 when moving away from the main welding interface 31 is the second rotation speed, which is greater than the first rotation speed.
[0112] The welding path 40 of the welding tool 20 includes a stable path 41 and a deviated path 42. The portion of the welding path 40 of the welding tool 20 along the main welding interface 31 is formed as the stable path 41, and the portion of the welding path 40 of the welding tool 20 deviating from the main welding interface 31 is formed as the deviated path 42. That is to say, the welding tool 20 rotates faster when moving along the deviated path 42, which can increase the number of stirring times of the material at the junction of the main welding interface 31 and the secondary welding interface 32, making the material stirring at this location more intense, which is beneficial to increase the uniformity of the material at this location, thereby improving the welding connection effect between multiple splicing interfaces 30, reducing the generation of defects, and thus ensuring the microstructure and mechanical properties of the weld.
[0113] In some embodiments, a ratio of the second rotation speed to the first rotation speed is β, 1<β<3.
[0114] For example, the ratio of the second rotation speed to the first rotation speed may be 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8 or any value between any two values therein, and the like.
[0115] The ratio of the second rotation speed to the first rotation speed is within this range. On the one hand, the second rotation speed will not be too large to increase the cost of the welding tool 20, and at the same time, the possibility of plastic deformation of the material around the junction of the main welding interface 31 and the secondary welding interface 32 caused by the excessive rotation speed of the welding tool 20 can be reduced; on the other hand, the number of stirring times of the material at the junction of the main welding interface 31 and the secondary welding interface 32 can be increased, so that the material at this location is stirred more violently, which is beneficial to increase the uniformity of the material at this location.
[0116] In some embodiments, when the deviation path 42 is a circular path, the maximum distance of the center of the welding tool 20 from the main welding interface 31 is 1 to 2 times the root diameter of the stirring pin 21. In other words, the maximum distance between the deviation path 42 and the main welding interface 31 in a direction perpendicular to the main welding interface 31 is 1 to 2 times the root diameter of the stirring pin 21.
[0117] For example, the maximum distance that the center of the welding tool 20 deviates from the main welding interface 31 can be 1 times, 1.2 times, 1.4 times, 1.6 times, 1.8 times, 2 times, or any value between any two of the root diameters of the stirring needle 21 .
[0118] The maximum distance that the center of the welding tool 20 deviates from the main welding interface 31 is not less than the root diameter of the stirring needle 21. In this way, along the direction of the secondary welding interface 32, the stirring needle 21 can completely deviate from the position when the stirring needle 21 is located at the main welding interface 31, so that the partial material connected to the secondary welding interface 32 and the main welding interface 31 can be stirred multiple times and the stirring direction is opposite, which is beneficial to the partial splicing interface 30 after the migration of the broken parts, and increases the mixing degree of the splicing interface 30 and the surrounding materials, thereby improving the microstructure and mechanical properties of the weld area and reducing the generation of hook defects. The maximum distance that the center of the welding tool 20 deviates from the main welding interface 31 is not more than twice the root diameter of the stirring needle 21. In this way, the distance that the welding tool 20 deviates from the main welding interface 31 will not be too far to increase the length of the welding path 40 too much, thereby reducing the welding production efficiency.
[0119] In some embodiments, when the deviation path 42 is an arc path, the maximum distance that the center of the welding tool 20 deviates from the main welding interface 31 does not exceed the radius of the root of the stirring needle 21 to reduce the impact on the effective welding width of the main welding interface 31.
[0120] See also Fig.15 In some embodiments, the welding method further comprises:
[0121] 05. When the welding tool 20 performs friction stir welding on the metal ring 3, the second metal layer 12 and the metal back plate 2, the friction stir welding area is heated and / or ultrasonic waves are emitted.
[0122] See also Figure 2 In some embodiments, the welding device 100 may further include an auxiliary module 150, and step 05 may be implemented by the auxiliary module 150, or in other words, the auxiliary module 150 may be used to heat and / or emit ultrasonic waves to the friction stir welding area when the welding tool 20 performs friction stir welding on the metal ring 3, the second metal layer 12 and the metal back plate 2.
[0123] Specifically, the auxiliary module 150 can heat only the friction stir welding area, the auxiliary module 150 can also emit ultrasonic waves only to the friction stir welding area, and the auxiliary module 150 can also heat the friction stir welding area and emit ultrasonic waves at the same time. It can be understood that heating the friction stir welding area can ensure the thermoplasticity of the welding material in the friction stir welding area, and then the welding material will migrate with the stirring needle 21 of the welding tool 20, thereby ensuring the welding strength, and emitting ultrasonic waves to the friction stir welding area can increase the temperature of the weld, thereby softening the welding material, and is conducive to reducing residual stress and welding deformation. In addition, ultrasonic vibration can improve the surface forming of the weld, reduce or even eliminate the hole defects caused by insufficient material flow.
[0124] The power range of the ultrasonic wave is 500-10000 watts. For example, the power of the ultrasonic wave can be 500 watts, 1000 watts, 2000 watts, 3000 watts, 5000 watts, 8000 watts or 10000 watts. The power of the ultrasonic wave is not limited and can be adjusted according to welding requirements. The heating temperature range is 30-10000°. For example, the heating temperature can be 30°, 100°, 200°, 500°, 1000°, 2000°, 5000° or 10000°. The heating temperature can be adjusted according to welding requirements and is not limited.
[0125] In this way, when the stirring needle 21 performs friction stir welding on the metal ring 3, the second metal layer 12 and the metal back plate 2, the friction stir welding area is heated and / or ultrasonic waves are emitted, which improves the welding quality and reduces the unqualified rate of the composite plate.
[0126] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0127] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
[0128] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A welding method, characterized in that: For forming a composite plate, the welding method comprises: Obtain a composite frame, a metal back plate and a metal ring, wherein the composite frame includes a first metal layer and a second metal layer, the first metal layer constitutes an outer wall of the composite frame, the second metal layer constitutes an inner wall of the composite frame, and the first metal layer and the second metal layer are made of different materials; The composite frame and the metal back plate are arranged on a welding table, wherein the metal back plate is located inside the composite frame and adjacent to the second metal layer; The metal ring cover is arranged on the composite frame; The metal ring, the second metal layer and the metal back plate are subjected to stir friction welding by a welding tool to form the composite plate.
2. The welding method according to claim 1, characterized in that: The metal ring includes multiple pieces, and the metal ring is covered on the composite frame, including: A plurality of metal rings are respectively covered on two opposite sides of the composite frame.
3. The welding method according to claim 1, characterized in that The method comprises welding the metal ring, the second metal layer and the metal back plate by the welding tool to form the composite plate, comprising: Performing friction stir welding on the metal ring, the second metal layer and the metal back plate by using the welding tool with a single-sided friction stir welding process to form the composite plate; or The metal ring, the second metal layer and the metal back plate are subjected to friction stir welding by using the welding tool with a double-sided friction stir welding process to form the composite plate.
4. The welding method according to claim 1, characterized in that: The metal ring, the second metal layer and the metal back plate are subjected to friction stir welding by the welding tool to form the composite plate, comprising: At least one splicing interface is used as a main welding interface, and the splicing interface connected to the main welding surface and located on the side of the main welding interface is used as a secondary welding interface; The welding tool is controlled to weld along the main welding interface and at least partially deviate from the main welding interface to weld toward the secondary welding interface, so as to form the composite plate.
5. The welding method according to claim 4, characterized in that: The portion of the welding tool welded along the main welding interface forms a stable path, and the portion of the welding tool that deviates from the main welding interface and welds offset to the secondary welding interface forms a deviated path, and the deviated path includes an arc path, an annular path, or a combination of one or more of the arc path, the annular path and a straight path.
6. The welding method according to claim 4, characterized in that: The speed of the welding tool when moving along the main welding interface is a first speed, and the speed of the welding tool when moving away from the main welding interface is a second speed, and the second speed is less than the first speed.
7. The welding method according to claim 4, characterized in that: The self-rotation speed of the welding tool when moving along the main welding interface is a first rotation speed, and the self-rotation speed of the welding tool when moving away from the main welding interface is a second rotation speed, and the second rotation speed is greater than the first rotation speed.
8. The welding method according to claim 5, characterized in that: The deviation path is an arc path, and the maximum distance that the center of the welding tool deviates from the main welding interface does not exceed the radius of the root of the stirring needle of the welding tool.
9. The welding method according to claim 1, characterized in that: The welding method further comprises: When the welding tool performs friction stir welding on the metal ring, the second metal layer and the metal back plate, heating and / or emitting ultrasonic waves are performed on the friction stir welding area.
10. The welding method according to claim 1, characterized in that: The type of the welding tool is dynamic shoulder / static shoulder.
11. The welding method according to claim 1, characterized in that: The metal ring is flush with the metal back plate.
12. A welding device, characterized in that: For forming a composite plate, the welding apparatus comprises: An acquisition module, used for acquiring a composite frame, a metal back plate and a metal ring, wherein the composite frame includes a first metal layer and a second metal layer, wherein the first metal layer constitutes an outer wall of the composite frame, and the second metal layer constitutes an inner wall of the composite frame, and the first metal layer and the second metal layer are made of different materials; An installation module, used for placing the composite frame and the metal back plate on a welding table, wherein the metal back plate is located inside the composite frame and adjacent to the second metal layer; A fixing module, used for placing the metal ring cover on the composite frame; The control module is used to stir friction welding the metal ring, the second metal layer and the metal back plate by using a welding tool to form the composite plate.