A green thermal insulation mortar material and its preparation method and application
By using cement, waste tungsten tailings powder, composite expanded vitrified microbeads and pineapple leaf fiber/resin composite materials in construction mortar materials, the problems of insufficient strength, poor insulation performance and environmental pollution in the prior art are solved. The preparation of green and environmentally friendly high-performance insulation mortar materials has been realized.
Patent Information
- Application Number
- CN202411110578.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing building mortar materials have insufficient tensile strength, limited insulation performance, poor durability and environmental pollution.
Cement is used as the cementitious material, combined with waste tungsten tailings powder, composite expanded vitrified microbeads and pineapple leaf fiber/resin composite materials, and good insulation properties are prepared through the synergistic effect of water reducing agent, defoaming agent and stabilizer. , green insulation mortar material with excellent mechanical properties and durability.
It significantly improves the insulation performance and mechanical properties of the mortar, reduces the preparation cost, solves the environmental pollution problem, and meets the waterproofness and strength requirements of special projects.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and specifically discloses a green thermal insulation mortar material, a preparation method and application thereof. Background Art
[0002] Thermal insulation mortar is a crucial functional material for achieving thermal insulation in building exterior walls. Traditional thermal insulation mortar is a premixed dry mortar made by mixing various lightweight materials as aggregates, cement as a binder, and some modified additives. However, its low water resistance and strength make it difficult to meet the requirements of some specialized projects. Therefore, improving thermal insulation mortar materials has become a key research topic for engineers.
[0003] Currently, there have been reports of improving the thermal insulation performance of insulation mortar materials by optimizing the raw material ratios, modifying the raw materials, or adding cellulose or phase change materials to reduce the thermal conductivity of the mortar aggregate. However, existing technologies still suffer from insufficient tensile strength, limited thermal insulation performance, poor durability, and environmental pollution. Therefore, developing a high-performance, environmentally friendly insulation mortar material is crucial for reducing building energy consumption. Summary of the Invention
[0004] To address the problems of insufficient tensile strength, limited thermal insulation performance, poor durability, and environmental pollution in the preparation process of existing building mortar materials, the present invention provides a green thermal insulation mortar material, its preparation method, and application. The green thermal insulation mortar material is prepared using cement as a gelling material; waste tungsten tailings powder, standard sand, composite expanded glass microspheres, and pineapple leaf fiber / resin composite materials as aggregates; and water reducers, defoamers, and stabilizers as additives. The present invention utilizes the synergistic effect of the various raw material components to ensure that the resulting green thermal insulation mortar material has good thermal insulation performance, excellent mechanical properties, and durability.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] A first aspect of the present invention provides a green thermal insulation mortar material, comprising the following raw material components in parts by weight: 100-120 parts of cement, 30-80 parts of waste tungsten tailings powder, 150-180 parts of standard sand, 1-2 parts of a water reducer, 0.5-1 parts of a defoamer, 0.05-0.1 parts of a stabilizer, 20-35 parts of composite expanded glass microspheres, 30-50 parts of a pineapple leaf fiber / resin reinforcement material, and 60-90 parts of water;
[0007] The composite expanded glass microspheres include expanded glass microspheres and dodecanol-modified silica aerogels attached to the surfaces of the expanded glass microspheres.
[0008] Expanded vitrified microspheres are a new green inorganic material with excellent resistance to high temperatures, frost, corrosion, and aging, and offer strong adhesion to building surfaces. The microspheres have a porous interior with high porosity, resulting in excellent fluidity, a minimal construction process, and consistent quality. However, the numerous open pores on their surface increase their water absorption and thermal conductivity, compromising the mortar's insulation and strength, leading to durability issues.
[0009] Silica aerogel has a high specific surface area and high porosity, with pore diameters smaller than the free path of air, resulting in extremely low thermal conductivity. Directly incorporating aerogel into mortar can cause aerogel agglomeration, creating significant gaps between the aerogel and the hydration products of the mortar, affecting the mortar's mechanical properties. More importantly, direct incorporation of aerogel into mortar requires a large amount of aerogel to maintain good thermal insulation properties, which can lead to high production costs.
[0010] Based on this, the present invention attaches silica aerogel to expanded glass microspheres with a porous structure, which not only fills the open pores on the surface of the expanded glass microspheres and repairs their surface defects, but also enhances the surface strength of the expanded glass microspheres to a certain extent. More importantly, the composite glass microspheres not only greatly reduce the thermal conductivity of the expanded glass microspheres, thereby improving the thermal insulation performance of the mortar material, but also effectively solves the problem that aerogel is unstable in mortar and the high cost caused by high dosage. The present invention also adds pineapple leaf fiber / resin composite materials to the mortar material, which effectively enhances the mechanical properties of the mortar material. Since the fiber cannot provide a conduction path for the heat energy in the resin material, the thermal conductivity and thermal diffusion coefficient of the resin composite material are further reduced, thereby improving the thermal insulation performance of the mortar material. Furthermore, the present invention also adds waste tungsten tailings powder, which not only effectively alleviates the processing pressure of the waste ore powder, but also further reduces the preparation cost of the mortar material.
[0011] Preferably, the preparation method of the composite expanded glass microspheres comprises the following steps:
[0012] S1. Heating the expanded vitrified microspheres to 200° C.-300° C. for heat treatment to obtain pretreated expanded vitrified microspheres;
[0013] S2. Dispersing ethyl orthosilicate and dodecanol in an alcohol solution, adjusting the pH to 2-3, adding a gel accelerator, and allowing to stand at 70° C.-90° C. for aging to obtain a mixed wet gel;
[0014] S3, adding the mixed wet gel to an organic solution containing silane and soaking it for 24 h to 48 h, washing it, and vacuum drying it to obtain dodecanol-modified silica aerogel powder;
[0015] S4. Dispersing the lauryl alcohol-modified silica aerogel powder in organic alcohol, adding the pretreated expanded vitrified microspheres, mixing evenly, filtering, and drying to obtain the composite expanded vitrified microspheres.
[0016] Further preferably, in S1, the temperature is increased by programmed temperature increase, and the rate of temperature increase is 5°C / min-10°C / min.
[0017] Further preferably, in S1, the holding time of the heat treatment is 4h-6h.
[0018] Further preferably, in S1, the particle size of the expanded glass microspheres is 0.5 mm-1 mm.
[0019] Further preferably, in S2, the mass ratio of the ethyl orthosilicate to dodecyl alcohol is 10:2-15:5.
[0020] Further preferably, in S2, the alcohol solution is an ethanol solution with a mass concentration of 70%-85%, and the mass volume ratio of the ethyl orthosilicate to the alcohol solution is 1g:2mL-1g:5mL.
[0021] Further preferably, in S2, the gel accelerator is propylene oxide.
[0022] Further preferably, in S2, the amount of the gel accelerator added is 0.5%-0.7% of the mass of the alcohol solution.
[0023] Further preferably, in S2, the static aging time is 14h-20h.
[0024] Further preferably, in S3, the organic solution containing silane is a n-hexane solution containing trimethylethoxysilane, wherein the volume ratio of the trimethylethoxysilane to n-hexane is 1:2-1:4.
[0025] Further preferably, in S3, the mass ratio of the mixed wet gel to the silane-containing organic solution is 1:2-1:4.
[0026] Further preferably, in S3, the washing is performed using n-hexane.
[0027] Further preferably, in S3, the vacuum drying temperature is 80° C.-90° C., and the vacuum drying time is 12 h-16 h.
[0028] More preferably, in S4, the organic alcohol is anhydrous ethanol.
[0029] Further preferably, in S4, the mass volume ratio of the dodecanol-modified silica aerogel powder to the organic alcohol is 1 g:3 mL to 1 g:5 mL.
[0030] Further preferably, in S4, the mass ratio of the dodecanol-modified silica aerogel powder to the pretreated expanded vitrified microspheres is 1:3-1:5.
[0031] Preferably, the preparation method of the pineapple leaf fiber / resin reinforced material comprises the following steps: immersing the pineapple leaf fiber in liquid phenolic resin, gradually heating the temperature to 160° C.-180° C. under an inert atmosphere, and keeping the temperature for 1 hour-3 hours to obtain the pineapple leaf fiber / resin reinforced material.
[0032] Further preferably, the mass volume ratio of the pineapple leaf fiber to the liquid phenolic resin is 1g:5mL-1g:8mL.
[0033] Further preferably, the specific operation of the gradient temperature increase is: using a programmed temperature increase method to increase the temperature to 80°C-100°C once, and keeping it warm for 2h-4h once; then using a programmed temperature increase method to increase the temperature to 120°C-140°C for a second time, and keeping it warm for 2h-4h twice, and finally increasing the temperature to 160°C-180°C by a programmed temperature increase method.
[0034] More preferably, the heating rate of the programmed temperature is 4°C / min-6°C / min.
[0035] Preferably, the cement is Portland cement.
[0036] Preferably, the particle size of the waste tungsten tailings powder is 0.3mm-0.8mm.
[0037] Preferably, the particle size of the standard sand is 0.5 mm-1 mm.
[0038] Preferably, the water reducer is a polycarboxylic acid high performance water reducer.
[0039] Preferably, the defoaming agent is any one of P803, A240 or BYK-012.
[0040] Preferably, the stabilizer is any one of EL0002, TAB-2 or T-386.
[0041] A second aspect of the present invention provides a method for preparing a green thermal insulation mortar material, comprising the following steps:
[0042] The raw material components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain a green thermal insulation mortar material.
[0043] The third aspect of the present invention provides an application of the green thermal insulation mortar material or the green thermal insulation mortar material prepared by the preparation method of the green thermal insulation mortar material in the field of building insulation.
[0044] In summary, the present invention provides a green thermal insulation mortar material, a preparation method and application thereof, wherein the green thermal insulation mortar material is prepared with cement as a gelling material; waste tungsten tailings powder, standard sand, composite expanded glass microspheres and pineapple leaf fiber / resin composite materials as aggregates; and a water reducer, a defoamer and a stabilizer as auxiliary agents. The present invention utilizes the synergistic effect of the raw material components to make the obtained green thermal insulation mortar material have good thermal insulation performance, excellent mechanical properties and durability, thereby effectively solving the problems of insufficient tensile strength, limited thermal insulation performance, poor durability and environmental pollution caused by the preparation process of the building mortar materials in the prior art. DETAILED DESCRIPTION
[0045] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.
[0046] Example 1
[0047] This embodiment provides a green thermal insulation mortar material and a preparation method thereof, which specifically includes the following contents:
[0048] The green thermal insulation mortar material includes the following raw material components in parts by mass: 120 parts of silicate cement, 60 parts of waste tungsten tailings powder, 170 parts of standard sand, 2 parts of polycarboxylic acid high-performance water reducer, 0.5 parts of defoamer P803, 0.1 parts of stabilizer EL0002, 25 parts of composite expanded glass microspheres, 40 parts of pineapple leaf fiber / resin reinforcement material and 70 parts of water.
[0049] The raw material components are weighed according to the designed ratio, and mixed evenly to obtain the green thermal insulation mortar material.
[0050] The preparation method of the composite expanded glass microspheres comprises the following steps:
[0051] S1. Heating 200 g of expanded vitrified microspheres with a particle size of 0.8 mm to 250° C. at a heating rate of 10° C. / min and keeping the temperature for 4 h to obtain pretreated expanded vitrified microspheres;
[0052] S2. Disperse 100 g of ethyl orthosilicate and 30 g of dodecanol in 300 mL of 75% ethanol solution, adjust the pH to 2.5, add 1.5 g of propylene oxide, and allow to stand at 75° C. for 16 h to obtain a mixed wet gel;
[0053] S3, adding the mixed wet gel to 500 g of a mixed solution of trimethylethoxysilane and n-hexane in a volume ratio of 1:3 and soaking for 36 h, washing with n-hexane twice, and vacuum drying at 85 ° C for 14 h to obtain 75.4 g of dodecanol-modified silica aerogel powder;
[0054] S4. Disperse the lauryl alcohol-modified silica aerogel powder in 300 mL of anhydrous ethanol, add the pretreated expanded vitrified microbeads, shake at room temperature in a water bath for 5 h, filter, and dry to obtain the composite expanded vitrified microbeads.
[0055] The preparation method of the pineapple leaf fiber / resin reinforced material comprises the following steps: impregnating pineapple leaf fiber in liquid phenolic resin, heating the pineapple leaf fiber to 90° C. at a heating rate of 5° C. / min under an inert atmosphere, keeping the temperature for 3 hours, then heating the pineapple leaf fiber to 130° C. at a heating rate of 5° C. / min, keeping the temperature for 3 hours, and finally heating the pineapple leaf fiber / resin reinforced material to 170° C. at a heating rate of 5° C. / min, keeping the temperature for 1.5 hours, to obtain the pineapple leaf fiber / resin reinforced material.
[0056] The particle size of the waste tungsten tailings powder is 0.5 mm.
[0057] The particle size of the standard sand is 0.8 mm.
[0058] Example 2
[0059] This embodiment provides a green thermal insulation mortar material and a preparation method thereof, which specifically includes the following contents:
[0060] The green thermal insulation mortar material includes the following raw material components in parts by mass: 120 parts of silicate cement, 60 parts of waste tungsten tailings powder, 160 parts of standard sand, 1 part of polycarboxylic acid high-performance water reducer, 0.5 parts of defoamer BYK-012, 0.1 parts of stabilizer T-386, 30 parts of composite expanded glass microspheres, 40 parts of pineapple leaf fiber / resin reinforcement material and 80 parts of water.
[0061] The raw material components are weighed according to the designed ratio, and mixed evenly to obtain the green thermal insulation mortar material.
[0062] The preparation method of the composite expanded glass microspheres comprises the following steps:
[0063] S1. Heating 200 g of expanded vitrified microspheres with a particle size of 0.6 mm to 250° C. at a heating rate of 10° C. / min and keeping the temperature for 5 h to obtain pretreated expanded vitrified microspheres;
[0064] S2. Disperse 100 g of ethyl orthosilicate and 30 g of dodecanol in 300 mL of 75% ethanol solution, adjust the pH to 2.5, add 1.5 g of propylene oxide, and allow to stand at 75° C. for 16 h to obtain a mixed wet gel;
[0065] S3, adding the mixed wet gel to 500 g of a mixed solution of trimethylethoxysilane and n-hexane in a volume ratio of 1:3 and soaking for 36 h, washing with n-hexane twice, and vacuum drying at 85 ° C for 14 h to obtain 75.4 g of dodecanol-modified silica aerogel powder;
[0066] S4. Disperse the lauryl alcohol-modified silica aerogel powder in 300 mL of anhydrous ethanol, add the pretreated expanded vitrified microbeads, shake at room temperature in a water bath for 5 h, filter, and dry to obtain the composite expanded vitrified microbeads.
[0067] The preparation method of the pineapple leaf fiber / resin reinforced material comprises the following steps: immersing pineapple leaf fiber in liquid phenolic resin, heating the mixture to 90°C at a heating rate of 5°C / min under an inert atmosphere, keeping the temperature for 3 hours, then heating the mixture to 130°C at a heating rate of 5°C / min, keeping the temperature for 3 hours, and finally heating the mixture to 170°C at a heating rate of 5°C / min, keeping the temperature for 2 hours, to obtain the pineapple leaf fiber / resin reinforced material.
[0068] The particle size of the waste tungsten tailings powder is 0.5 mm.
[0069] The particle size of the standard sand is 0.8 mm.
[0070] Example 3
[0071] This embodiment provides a green thermal insulation mortar material and a preparation method thereof, which specifically includes the following contents:
[0072] The green thermal insulation mortar material includes the following raw material components in parts by mass: 117 parts of Portland cement, 75 parts of waste tungsten tailings powder, 152 parts of standard sand, 1.2 parts of polycarboxylic acid high-performance water reducer, 0.6 parts of defoamer A240, 0.06 parts of stabilizer TAB-2, 35 parts of composite expanded glass microspheres, 50 parts of pineapple leaf fiber / resin reinforcement material and 80 parts of water.
[0073] The raw material components are weighed according to the designed ratio, and mixed evenly to obtain the green thermal insulation mortar material.
[0074] The preparation method of the composite expanded glass microspheres comprises the following steps:
[0075] S1. Heating 200 g of expanded vitrified microspheres with a particle size of 0.7 mm to 250° C. at a heating rate of 10° C. / min and keeping the temperature for 6 h to obtain pretreated expanded vitrified microspheres;
[0076] S2. Disperse 100 g of ethyl orthosilicate and 30 g of dodecanol in 300 mL of 75% ethanol solution, adjust the pH to 2.5, add 1.5 g of propylene oxide, and allow to stand at 75° C. for 16 h to obtain a mixed wet gel;
[0077] S3, adding the mixed wet gel to 500 g of a mixed solution of trimethylethoxysilane and n-hexane in a volume ratio of 1:3 and soaking for 36 h, washing with n-hexane twice, and vacuum drying at 85 ° C for 14 h to obtain 75.4 g of dodecanol-modified silica aerogel powder;
[0078] S4. Disperse the lauryl alcohol-modified silica aerogel powder in 300 mL of anhydrous ethanol, add the pretreated expanded vitrified microbeads, shake at room temperature in a water bath for 5 h, filter, and dry to obtain the composite expanded vitrified microbeads.
[0079] The preparation method of the pineapple leaf fiber / resin reinforced material comprises the following steps: impregnating pineapple leaf fiber in liquid phenolic resin, heating the mixture to 90°C at a heating rate of 5°C / min under an inert atmosphere, keeping the temperature for 3 hours, then heating the mixture to 130°C at a heating rate of 5°C / min, keeping the temperature for 3 hours, and finally heating the mixture to 170°C at a heating rate of 5°C / min, keeping the temperature for 3 hours, to obtain the pineapple leaf fiber / resin reinforced material.
[0080] The particle size of the waste tungsten tailings powder is 0.5 mm.
[0081] The particle size of the standard sand is 0.8 mm.
[0082] Comparative Example 1
[0083] This comparative example provides a green thermal insulation mortar material and a preparation method thereof. The difference from Example 1 is that the composite expanded vitrified microspheres are expanded vitrified microspheres filled with silica aerogel, and other components and processes remain unchanged. Specifically, the following contents are included:
[0084] The green thermal insulation mortar material includes the following raw material components in parts by mass: 120 parts of silicate cement, 60 parts of waste tungsten tailings powder, 170 parts of standard sand, 2 parts of polycarboxylic acid high-performance water reducer, 0.5 parts of defoamer P803, 0.1 parts of stabilizer EL0002, 25 parts of composite expanded glass microspheres, 40 parts of pineapple leaf fiber / resin reinforcement material and 70 parts of water.
[0085] The raw material components are weighed according to the designed ratio, and mixed evenly to obtain the green thermal insulation mortar material.
[0086] The preparation method of the composite expanded glass microspheres comprises the following steps:
[0087] S1. Heating 200 g of expanded vitrified microspheres with a particle size of 0.8 mm to 250° C. at a heating rate of 10° C. / min and keeping the temperature for 4 h to obtain pretreated expanded vitrified microspheres;
[0088] S2. Disperse 100 g of ethyl orthosilicate in 300 mL of 75% ethanol solution, adjust the pH to 2.5, add 1.5 g of propylene oxide, and age at 75° C. for 16 h to obtain a mixed wet gel;
[0089] S3, adding the mixed wet gel to 500 g of a mixed solution of trimethylethoxysilane and n-hexane in a volume ratio of 1:3 and soaking for 36 h, washing with n-hexane twice, and vacuum drying at 85 ° C for 14 h to obtain 61.3 g of silica aerogel powder;
[0090] S4. Disperse the silica aerogel powder in 300 mL of anhydrous ethanol, add the pretreated expanded vitrified microbeads, shake at room temperature in a water bath for 5 h, filter, and dry to obtain the composite expanded vitrified microbeads.
[0091] The preparation method of the pineapple leaf fiber / resin reinforced material comprises the following steps: impregnating pineapple leaf fiber in liquid phenolic resin, heating the pineapple leaf fiber to 90° C. at a heating rate of 5° C. / min under an inert atmosphere, keeping the temperature for 3 hours, then heating the pineapple leaf fiber to 130° C. at a heating rate of 5° C. / min, keeping the temperature for 3 hours, and finally heating the pineapple leaf fiber / resin reinforced material to 170° C. at a heating rate of 5° C. / min, keeping the temperature for 1.5 hours, to obtain the pineapple leaf fiber / resin reinforced material.
[0092] The particle size of the waste tungsten tailings powder is 0.5 mm.
[0093] The particle size of the standard sand is 0.8 mm.
[0094] Comparative Example 2
[0095] This comparative example provides a green thermal insulation mortar material and a preparation method thereof. The difference from Example 1 is that the pineapple leaf fiber / resin reinforcement material is not included, and other components and processes remain unchanged. Specifically, the following contents are included:
[0096] The green thermal insulation mortar material includes the following raw material components in parts by mass: 120 parts of silicate cement, 60 parts of waste tungsten tailings powder, 170 parts of standard sand, 2 parts of polycarboxylic acid high-performance water reducer, 0.5 parts of defoamer P803, 0.1 parts of stabilizer EL0002, 25 parts of composite expanded vitrified microspheres and 70 parts of water.
[0097] The raw material components are weighed according to the designed ratio, and mixed evenly to obtain the green thermal insulation mortar material.
[0098] The preparation method of the composite expanded glass microspheres comprises the following steps:
[0099] S1. Heating 200 g of expanded vitrified microspheres with a particle size of 0.8 mm to 250° C. at a heating rate of 10° C. / min and keeping the temperature for 4 h to obtain pretreated expanded vitrified microspheres;
[0100] S2. Disperse 100 g of ethyl orthosilicate and 30 g of dodecanol in 300 mL of 75% ethanol solution, adjust the pH to 2.5, add 1.5 g of propylene oxide, and allow to stand at 75° C. for 16 h to obtain a mixed wet gel;
[0101] S3, adding the mixed wet gel to 500 g of a mixed solution of trimethylethoxysilane and n-hexane in a volume ratio of 1:3 and soaking for 36 h, washing with n-hexane twice, and vacuum drying at 85 ° C for 14 h to obtain 75.4 g of dodecanol-modified silica aerogel powder;
[0102] S4. Disperse the lauryl alcohol-modified silica aerogel powder in 300 mL of anhydrous ethanol, add the pretreated expanded vitrified microbeads, shake at room temperature in a water bath for 5 h, filter, and dry to obtain the composite expanded vitrified microbeads.
[0103] The particle size of the waste tungsten tailings powder is 0.5 mm.
[0104] The particle size of the standard sand is 0.8 mm.
[0105] In order to further demonstrate the technical effects of the present invention, the present invention conducted the following tests on the mortar materials obtained in Examples 1-3 and Comparative Examples 1-2: the compressive strength and flexural strength were tested with reference to the standard of GB / T17671-2021, and the thermal conductivity was measured using a JW-Ⅲ heat flow meter-type thermal conductivity meter and a device for measuring thermal conductivity using a thermal pulse method. The results are shown in Table 1.
[0106] Table 1 Performance test results of various mortar materials
[0107]
[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A green thermal insulation mortar material, characterized by: The raw material components include the following parts by weight: 100-120 parts of cement, 30-80 parts of waste tungsten tailings powder, 150-180 parts of standard sand, 1-2 parts of water reducer, 0.5-1 parts of defoamer, 0.05-0.1 parts of stabilizer, 20-35 parts of composite expanded glass microspheres, 30-50 parts of pineapple leaf fiber / resin reinforcement material and 60-90 parts of water; The composite expanded vitrified microspheres include expanded vitrified microspheres and dodecanol-modified silica aerogels attached to the surfaces of the expanded vitrified microspheres; The preparation method of the composite expanded vitrified microspheres comprises the following steps: S1, heating the expanded vitrified microspheres to 200°C-300°C for heat treatment to obtain pretreated expanded vitrified microspheres; S2, dispersing tetraethyl orthosilicate and dodecanol in an alcohol solution, adjusting the pH to 2-3, adding a gel accelerator, and standing and aging at 70° C.-90° C. to obtain a mixed wet gel; S3, adding the mixed wet gel into an organic solution containing silane and soaking it for 24h-48h, washing it, and vacuum drying it to obtain dodecanol modified silica aerogel powder; S4, dispersing the lauryl alcohol modified silica aerogel powder in organic alcohol, adding the pretreated expanded vitrified microspheres, mixing evenly, filtering, and drying to obtain the composite expanded vitrified microspheres; The preparation method of the pineapple leaf fiber / resin reinforced material comprises the following steps: immersing the pineapple leaf fiber in liquid phenolic resin, gradually heating to 160° C.-180° C. in an inert atmosphere, and keeping the temperature for 1 h-3 h to obtain the pineapple leaf fiber / resin reinforced material.
2. The green thermal insulation mortar material according to claim 1, characterized in that: In S1, the temperature is increased by programmed temperature increase, and the rate of temperature increase is 5°C / min-10°C / min; and / or In S1, the heat treatment holding time is 4h-6h; and / or In S1, the particle size of the expanded vitrified microspheres is 0.5 mm-1 mm.
3. The green thermal insulation mortar material according to claim 1, characterized in that: In S2, the mass ratio of tetraethyl orthosilicate to dodecanol is 10:2-15:5; and / or In S2, the alcohol solution is an ethanol solution with a mass concentration of 70%-85%, and the mass volume ratio of the tetraethyl orthosilicate to the alcohol solution is 1g:2mL-1g:5mL; and / or In S2, the gel accelerator is propylene oxide; and / or In S2, the static aging time is 14h-20h.
4. The green thermal insulation mortar material according to claim 1, characterized in that: In S3, the organic solution containing silane is a n-hexane solution containing trimethylethoxysilane, wherein the volume ratio of the trimethylethoxysilane to n-hexane is 1:2-1:4; and / or In S3, the mass ratio of the mixed wet gel to the silane-containing organic solution is 1:2-1:4; and / or In S3, the washing is performed using n-hexane.
5. The green thermal insulation mortar material according to claim 1, characterized in that: In S4, the mass volume ratio of the dodecanol modified silica aerogel powder to the organic alcohol is 1g:3mL-1g:5mL; and / or In S4, the mass ratio of the dodecanol modified silica aerogel powder to the pretreated expanded vitrified microspheres is 1:3-1:
5.
6. The green thermal insulation mortar material according to claim 1, characterized in that: The mass volume ratio of the pineapple leaf fiber to the liquid phenolic resin is 1g:5mL-1g:8mL; and / or The specific operation of the gradient heating is: heating to 80°C-100°C once by programmed heating, and keeping warm for 2h-4h; then heating to 120°C-140°C for a second time by programmed heating, and keeping warm for 2h-4h for a second time, and finally heating to 160°C-180°C by programmed heating.
7. The method for preparing the green thermal insulation mortar material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: weighing various raw material components according to the designed proportion, and evenly mixing the weighed components to obtain a green thermal insulation mortar material.
8. Application of the green thermal insulation mortar material according to any one of claims 1 to 6 or the green thermal insulation mortar material prepared by the preparation method of the green thermal insulation mortar material according to claim 7 in the field of building thermal insulation.