A method for preparing ceramic material from boron carbide grinding waste and its application

The problem of using boron carbide abrasive waste by ball milling or acid leaching is solved by using hot press sintering method, and high hardness and high toughness ceramic materials are prepared, suitable for wear-resistant and bulletproof applications, avoiding Resource waste and environmental pollution have improved material performance and economic value.

CN118637919BActive Publication Date: 2024-11-08NORTHEASTERN UNIV CHINA
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411087181.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Due to the small particles and high impurity content of boron carbide abrasive waste, the grinding efficiency is low and easy to scratch. There is currently no effective recycling method, resulting in waste of resources and environmental pollution.

Method used

Modified boron carbide grinding waste is treated by ball milling or acid leaching, and high hardness and high toughness boron carbide ceramic materials are prepared by hot press sintering method, and the material performance is improved by using the sintering effect of alumina.

Benefits of technology

It realizes the high hardness and toughness of boron carbide ceramic materials, is suitable for wear-resistant structural materials and bulletproof armor, avoids solid waste accumulation, creates economic value, and significantly improves the performance and service life of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a method for preparing ceramic materials from boron carbide grinding waste and its application, belonging to the technical field of preparing ceramics by comprehensive utilization of secondary resources. The method comprises pre-treating the waste, ball milling or acid leaching the pre-treated grinding waste to obtain modified waste, and hot pressing and sintering the modified waste to obtain ceramic materials. The present invention realizes the recycling of waste resources and turns waste into treasure, which not only protects the environment but also has high economic value. The ceramic material prepared by sintering has excellent performance, meets market standards, and has outstanding hardness and toughness. It can be applied to fields such as wear-resistant structural materials in the civilian field, and can be applied to fields such as bulletproof vests and bulletproof armor in the military field. It is simple and feasible to operate, low cost, and convenient for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparing ceramics by comprehensive utilization of secondary resources, and specifically relates to a method for preparing ceramics by using boron carbide grinding waste and application thereof. Background Art

[0002] With the increasing maturity of single crystal growth technology and processing technology, the application of sapphire in LED lighting, mobile phone cameras and screens, medical equipment, environmental protection and other industries is becoming more and more popular. When sapphire is used in the above fields, it must be ground and polished to achieve the flatness requirements of the application. Traditional grinding uses diamond as an abrasive to grind sapphire, but diamond is expensive and the grinding effect is average. Boron carbide (B4C) has a hardness between diamond and sapphire. It is relatively cheaper than diamond and has excellent grinding effect. Therefore, B4C powder is currently used in the industry to polish sapphire wafers. The polishing method adopts a free grinding method. As the grinding time increases, the grinding efficiency and quality of the B4C abrasive will no longer meet the requirements due to reasons such as particle breakage and size change. This batch of abrasives will be eliminated, thus forming B4C grinding waste. B4C grinding waste has the following characteristics: first, the particles are fine. Sapphire grinding and polishing belongs to the final finishing process of the process. The B4C abrasive itself has a fine particle size, and the B4C particles are further refined due to mechanical grinding. Secondly, it contains impurities. The ground sapphire enters the B4C abrasive. The main component of sapphire is Al2O3, so the main impurity in B4C grinding waste is Al2O3.

[0003] The B4C grinding waste has low grinding efficiency and is easy to scratch the polished surface when reused as abrasive. There is currently no effective method for its recycling. Summary of the invention

[0004] In order to solve the above technical problems, after studying and analyzing the properties of B4C grinding waste, it is believed that the fine particle size of B4C grinding waste has high surface energy and is suitable for sintering. Al2O3 can play a role in assisting the sintering of B4C at an appropriate addition amount. In view of the characteristics of B4C grinding waste, this application adopts ball milling, mixing or acid leaching to first modify the B4C grinding waste, and then uses hot pressing sintering to prepare the B4C grinding waste into a high-hardness, high-toughness B4C ceramic material. The obtained B4C ceramic material can be used in the field of wear-resistant structural materials, such as knives, bearings, nozzles, etc. in the civilian field, and can be used in the fields of bulletproof vests and bulletproof armor in the military field. In the civilian field, high hardness can improve the cutting ability of B4C tools, and high hardness can improve wear resistance and increase the tolerance of B4C bearings and nozzles. High toughness can reduce the probability of brittle fracture of B4C tools, bearings, and nozzles, making them less likely to break and fragment, and increase service life. In the military field, high hardness can improve the ability of B4C bulletproof ceramics to destroy warheads and weaken the penetration ability of bullets, and high toughness can significantly improve the ability of B4C bulletproof ceramics to resist multiple bullet attacks.

[0005] The method of the present invention is used to prepare B4C grinding waste into B4C ceramic material with high hardness and high toughness, which can not only avoid the environmental pollution problem caused by the accumulation of solid waste, but also turn waste into treasure, increase the value of waste and reuse it to create higher economic value.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing boron carbide ceramic material from boron carbide grinding waste comprises the following steps;

[0008] S1 Pretreatment: Remove larger debris from the waste by screening or selection, and grind the waste in a mortar;

[0009] S2 Modify the pre-treated waste by any of the following methods:

[0010] (1) The pretreated waste is subjected to ball milling treatment: the ball-to-material mass ratio is 3-6:1, the ball milling time is 7-12 h, and the ball milling speed is 200-450 r / min;

[0011] (2) performing conventional acid leaching or microwave acid leaching on the pretreated waste: the acid solution used is one or more of H2SO4 solution and HCl solution; the conventional acid leaching temperature is 90°C to 250°C; the microwave acid leaching temperature is 90°C to 240°C;

[0012] S3 hot pressing and sintering: drying the material obtained in S2 and hot pressing and sintering;

[0013] The mass percentage of aluminum oxide in the waste material is 8-22 wt %. Further, the mass percentage of aluminum oxide in the waste material is 8-13 wt %.

[0014] The waste material is boron carbide grinding waste used for fine grinding or polishing of sapphire.

[0015] The ball milling in S2 is carried out by dry or wet ball milling; when wet ball milling is adopted, ethanol is used as the medium, and the mass ratio of ethanol to the pretreated waste is 3.5~6.5:1.

[0016] In S2, ZrO2 or B4C balls are used for ball milling.

[0017] The mass concentration of the acid solution in S2 is 20%~50%, and the mass ratio of the volume of the acid solution to the pretreated waste is 3~10:1 mL / g.

[0018] The microwave power of microwave acid leaching treatment in S2 is 20~90 kW.

[0019] The heating rate of microwave acid leaching treatment in S2 is 5~15℃ / min.

[0020] The hot pressing sintering process in S3 includes heating to 1900~2100℃ at a rate of 20~30℃ / min, then pressurizing to a pressure of 15~60 MPa, and maintaining the temperature and pressure for 10~40 min. Further, when the temperature rises to 1900~2100℃, pressurizing to 15~60 MPa at a rate of 3~20 MPa / s.

[0021] The invention also provides application of the boron carbide ceramic material obtained by the method in bulletproof vests and bulletproof armor.

[0022] The present invention also provides the use of the boron carbide ceramic material obtained by the method in wear-resistant structural materials. The wear-resistant material includes a tool, a bearing and a nozzle.

[0023] Beneficial effects of the present invention:

[0024] (1) It realizes the recycling of waste resources and turns waste into treasure, which not only protects the environment but also has high economic value.

[0025] (2) The ceramic materials prepared by sintering have excellent performance, meet market standards, and have outstanding hardness and toughness. In the civilian field, they can be used in fields such as wear-resistant structural materials, and in the military field, they can be used in fields such as bulletproof vests and bulletproof armor.

[0026] (3) In the process of ball milling pretreatment, the present application obtains a boron carbide ceramic material with high hardness and excellent toughness at a high Al2O3 content. The waste materials themselves are mutually ground materials. Grinding can activate the powder, increase the surface energy of the powder, and increase the structural defects of the powder, so that the powder does not strictly meet the stoichiometric ratio, thereby promoting diffusion and densification during the sintering process. The activity of B4C grinding waste itself is higher than that of general powder. Secondly, this process performs targeted ball milling and dispersion to further activate the powder, break up the agglomerated B4C and Al2O3, form smaller particles, and improve uniformity. With the promotion of these two aspects, the hardness and toughness of the ceramic material obtained by sintering are improved compared with commercial pure powder, and the toughness is significantly improved.

[0027] (4) Based on the high activity of the B4C grinding waste itself, appropriate acid leaching treatment is carried out to form smaller particles and improve the uniformity of the particles, thereby obtaining a boron carbide ceramic material with both high hardness and excellent toughness.

[0028] (5) The operation is simple and feasible, the cost is low, and it is convenient for industrial production. DETAILED DESCRIPTION

[0029] In order to make the present invention more clear, the present invention is further described in detail below in conjunction with specific examples. It should be understood that the specific implementation cases described here are only used to explain the present invention and are not used to limit the present invention.

[0030] In the examples of the present invention, the bending strength is measured by a three-point bending method using an electronic universal mechanical testing machine.

[0031] In the examples of the present invention, the hardness is measured by the Vickers hardness method using a micro Vickers hardness tester.

[0032] In the examples of the present invention, the fracture toughness is measured using an indentation method.

[0033] The boron carbide grinding waste used in this embodiment has a composition of B4C 87.32 wt%, Al2O3 10.92 wt%, and others 1.76 wt%, and the median particle size of the waste is 3.3 μm. Example 1

[0034] Take 10 g of boron carbide grinding waste, use wet ball milling to mix, use ZrO2 balls, the ball-to-material mass ratio is 4:1, ethanol is the mixing medium, and the mass ratio of ethanol to material is 4:1. The ball milling time is 10 h, and the ball milling speed is 350 r / min. The material is dried at 80℃ in a vacuum oven for 4 h. At this time, the median particle size of the boron carbide grinding waste is 1.85μm, and then hot-pressed sintering is carried out, with a heating rate of 30℃ / min to 2000℃, and then pressurized, with a pressurization rate of 15 MPa / s, a pressure of 20 MPa, and heat preservation and pressure maintenance for 30 min. The obtained ceramic is well formed, with a hardness of 32 GPa, a flexural strength of 450 MPa, and a fracture toughness of 4.8 MPa·m 1 / 2 . Example 2

[0035] Take 10 g of boron carbide grinding waste and modify it by microwave acid leaching method, with H2SO4 mass concentration of 35%, liquid-solid ratio of 6 mL / g, heating rate of 8℃ / min, temperature of 240℃, and power of 50 kW. The material was dried in a vacuum oven at 80℃ for 4 h. At this time, the median particle size of boron carbide grinding waste was 1.75μm. Then it was hot-pressed and sintered at a heating rate of 30℃ / min to 2000℃, and then pressurized at a pressurization rate of 15 MPa / s and a pressure of 20 MPa. The ceramic was well formed, with about 2.5 wt% Al2O3 remaining, a hardness of 29.5 GPa, a flexural strength of 380 MPa, and a fracture toughness of 4.2 MPa·m 1 / 2 . Example 3

[0036] Take 10 g of boron carbide grinding waste and modify it by conventional acid leaching method, with H2SO4 mass concentration of 35%, liquid-solid ratio of 6 mL / g, heating rate of 8℃ / min, and temperature of 150℃. Dry the material in a vacuum oven at 80℃ for 4 h. At this time, the median particle size of the boron carbide grinding waste is 1.98 μm. Then hot press sintering is carried out, heating at a rate of 30℃ / min to 2000℃, and then pressurized at a rate of 15 MPa / s and a pressure of 20 MPa, and heat and pressure are maintained for 30 min. The obtained ceramic is well formed, with Al2O3 remaining about 7wt%, hardness of 30.8 GPa, bending strength of 410 MPa, and fracture toughness of 4.46MPa·m 1 / 2 .

[0037] Comparative Example 1

[0038] Take 10 g of boron carbide grinding waste and directly perform hot pressing sintering, heating up to 2000℃ at a rate of 30℃ / min, then pressurizing at a rate of 15 MPa / s and a pressure of 20 MPa for 30 min. The obtained ceramics quickly break under slight external force, and the molding and consolidation are not firm.

[0039] Comparative Example 2

[0040] Take 9g of boron carbide (median particle size of 1.33 microns), add 1g of Al2O3 to it, mix well, and use wet ball milling to mix the materials. Use ZrO2 balls, the ball-to-material mass ratio is 4:1, ethanol is used as the mixing medium, and the ethanol-to-material mass ratio is 4:1. The ball milling time is 10 h, and the ball milling speed is 350 r / min. The material is hot-pressed and sintered in the drying process, and the temperature is increased to 2000℃ at a rate of 30℃ / min, and then pressurized at a pressurization rate of 15 MPa / s and a pressure of 20 MPa, and the temperature is kept at 30 min. The obtained ceramic is well formed and has a toughness of 3.6MPa·m 1 / 2 , hardness 30.3 GPa.

Claims

1. A method for preparing ceramic materials from boron carbide grinding waste, characterized in that: The method comprises the following steps: S1 Pretreatment: Remove larger debris from the waste by screening or selection, and grind the waste in a mortar; S2 Modify the pre-treated waste by any of the following methods: (1) The pretreated waste is subjected to ball milling treatment: the ball-to-material mass ratio is 3-6:1, the ball milling time is 7-12 h, and the ball milling speed is 200-450 r / min; (2) performing conventional acid leaching or microwave acid leaching on the pretreated waste: the acid solution used is one or more of H2SO4 solution and HCl solution; the conventional acid leaching temperature is 90°C to 250°C; the microwave acid leaching temperature is 90°C to 240°C; S3 hot pressing and sintering: drying the material obtained in S2, and hot pressing and sintering to obtain boron carbide ceramics; The mass percentage of aluminum oxide in the waste is 8~22wt%; The mass concentration of the acid solution in S2 is 20% to 50%, and the mass ratio of the volume of the acid solution to the pretreated waste is 3 to 10:1 mL / g; The hot pressing sintering process in S3 includes heating up to 1900~2100°C at a rate of 20~30°C / min, followed by pressurization at a pressure of 15~60 MPa, and maintaining the temperature and pressure for 10~40 min.

2. The method for preparing ceramic material from boron carbide grinding waste as claimed in claim 1, characterized in that: The waste material is boron carbide grinding waste used for fine grinding or polishing of sapphire.

3. The method for preparing ceramic material from boron carbide grinding waste as claimed in claim 1, characterized in that: The ball milling in S2 is carried out by dry or wet ball milling; when wet ball milling is adopted, ethanol is used as the medium, and the mass ratio of ethanol to the pretreated waste is 3.5~6.5:

1.

4. The method for preparing ceramic material from boron carbide grinding waste as claimed in claim 1, characterized in that: The microwave power in S2 is 20~90 kW.

5. A method for preparing ceramic material from boron carbide grinding waste as claimed in claim 1 or 4, characterized in that: The heating rate of microwave acid leaching treatment in S2 is 5~15℃ / min.

6. Use of the ceramic material obtained by the method of claim 1 in bulletproof vests and bulletproof armor.

7. Use of the ceramic material obtained by the method according to claim 1 in wear-resistant structural materials.

Citation Information

Cited By

  • Superconducting Ketjen black / boron carbide composite ceramic and preparation method and application thereof

    CN119977582A