Construction material for seamless expansion joint of bridge and tunnel and construction method thereof

By using modified asphalt and polymer modifiers in seamless expansion joint materials, combined with high-temperature curing reaction and multi-layer paving methods, the problem of seamless expansion joint materials being easily damaged under high traffic flow is solved, and the problem of seamless expansion joint materials being easily damaged under high traffic flow is improved. Adhesion and durability meet the stability and durability requirements of bridge and tunnel engineering.

CN118638512BActive Publication Date: 2024-11-19JIANGSU RIVENDELL TRANSPORTATION TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411088850.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing seamless expansion joint materials are easily damaged under high traffic flow, have poor anti-aging properties and high-temperature thermal stability, and have poor adhesion to the cement paving interface, resulting in insufficient stability and durability.

Method used

Using cementitious materials including matrix asphalt, chemical modifiers, polymer modifiers, rubber powders and reinforcers, combined with primer of 801 glue and synergist, a strong bonding force is formed through high-temperature curing reaction, combined with multi-layer paving Installation method to improve adhesion and stability.

Benefits of technology

It significantly improves the stability and durability of seamless expansion joints, enhances the adhesion with the cement paving interface, extends the service life, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a construction material for seamless expansion joints of bridges and tunnels and a construction method thereof, and belongs to the field of road construction and maintenance. The construction materials include a binder and a primer, and the binder includes the following raw materials in parts by weight: 100 parts of matrix asphalt, 0.5-1 parts of chemical modifier, 3-5 parts of polymer modifier, 25-40 parts of rubber powder, and 5-15 parts of reinforcing agent; the primer is composed of 801 glue and synergist, and the mass ratio of 801 glue to synergist is 10:1-3; the mass ratio of synergist to reinforcing agent is 1:5. The construction method includes: grooving; brushing all wall surfaces in the trough body with the primer; heating the binder, mixing it with stone and stirring it evenly to obtain a mixture; paving the mixture into the trough body and cooling it down. The present invention utilizes a combination of a reinforcing agent and a synergist, and cooperates with the viscosity of 801 glue to minimize the possibility of "unsealing" of the contact surface, thereby extending the service life of the seamless expansion joint as a whole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of bridge and tunnel engineering, and in particular to a construction material for seamless expansion joints of bridges and tunnels and a construction method thereof. Background Art

[0002] An expansion joint is a structural joint set at an appropriate position along the construction joint direction of a building or structure to prevent cracks or damage to the building components due to climate temperature changes (thermal expansion and contraction). A seamless expansion joint is a structure in which elastic materials are filled in the expansion gap at the end of the bridge and waterproof materials are laid, and then viscoelastic composite materials are laid on the bridge deck pavement layer, so that the bridge deck pavement at the expansion joint forms a continuum with other pavement parts, and the deformation of materials such as asphalt concrete in the joint withstands expansion and contraction.

[0003] Compared with other types of expansion joints, seamless expansion joints can provide a sound surface for the building structure, resist damage to the structure by water or harmful components, and adapt to shrinkage caused by temperature. They have good integrity, durability, drainage performance, easy maintenance and repair, low noise and other advantages, and are widely used at home and abroad.

[0004] The seamless expansion joint technology currently on the market generally has poor anti-aging performance and poor high-temperature thermal stability. It is easily damaged by wheel rolls or lateral extrusion to form depressions under heavy traffic. At the same time, since the seamless expansion joint material itself is a semi-flexible material, mainly organic materials; and the surrounding bridge deck pavement is a rigid material, mostly inorganic materials such as cement; the cohesive force of the two is quite different, so the interface between the two is often "debonded" due to poor adhesion. Therefore, how to improve the stability and durability of seamless expansion joints under high traffic flow is an urgent problem that needs to be solved in the industry. Summary of the invention

[0005] In order to improve the deficiencies of the above-mentioned prior art, the present application provides a construction material for seamless expansion joints of bridges and tunnels and a construction method thereof, aiming to improve the stability of the seamless expansion joints and their adhesion to the interface with cement paving.

[0006] In the first aspect, the present application provides a construction material for seamless expansion joints of bridges and tunnels, which adopts the following technical solution:

[0007] A construction material for seamless expansion joints of bridges and tunnels, comprising a binder and a primer, wherein the binder comprises the following raw materials in parts by weight: 100 parts of base asphalt, 0.5-1 parts of a chemical modifier, 3-5 parts of a polymer modifier, 25-40 parts of rubber powder, and 5-15 parts of a reinforcing agent;

[0008] The primer is composed of 801 glue and a synergist, and the mass ratio of the 801 glue to the synergist is 10:1-3;

[0009] The mass ratio of the synergist to the enhancer is 1:5;

[0010] The chemical modifier is one or more of phosphoric acid, pyrophosphoric acid, and polyphosphoric acid;

[0011] The polymer modifier is one or both of styrene-isoprene block copolymer and styrene-butadiene block copolymer;

[0012] The reinforcing agent is E41 type epoxy resin, and the synergist is ultra-fine powdered dicyandiamide.

[0013] Specifically, the reinforcing agent is E41 epoxy resin, and the synergist is ultrafine powdered dicyandiamide, and the two can undergo a curing reaction under the promotion of high temperature. Therefore, the present application mixes the binder with the stone, and then paves it in a pre-opened slot. The reinforcing agent in the binder contacts the synergist in the primer, and a curing reaction occurs under the promotion of high temperature. The curing reaction is most in-depth at the interface where the slot and the binder contact, and a strong bonding force can be formed; at the same time, combined with the bonding property of the 801 glue itself, the possibility of "debonding" on the contact surface can be avoided to the greatest extent, and the overall service life of the seamless expansion joint can be extended.

[0014] Among the above components of the present application, the base asphalt can be selected from No. 70 petroleum base asphalt or No. 90 petroleum base asphalt; by adding a chemical modifier to the base asphalt, it can react with the asphaltene in the base asphalt to improve the high temperature performance of the asphalt. Specifically, the chemical modifier can not only increase the acid value of the base, improve the coating of asphalt with cement concrete, but also increase the softening point of asphalt and improve the high temperature stability of asphalt.

[0015] Moreover, the rubber powder in the above components is specifically 40-80 mesh waste tire rubber powder, which can absorb the light oil in the matrix asphalt and swell. Therefore, after adding the rubber powder, the content of light components in the asphalt is relatively reduced, and the asphalt colloids contain oil substances, so that the rubber particles will develop into a sol-gel structure to varying degrees, thereby improving the stretchability and compressibility of the asphalt.

[0016] At the same time, the chemical modifier added can greatly improve the swelling rate of rubber powder and obtain better modification effect. Chemical modifiers can form chemical reactions inside asphalt molecules to enhance the fluidity and viscosity of asphalt, improve its crack resistance and temperature stability. Moreover, as an environmentally friendly material, chemical modifiers can reduce the petroleum content of asphalt mixtures, thereby reducing its pollution and impact on the environment.

[0017] By adding polymer modifiers to the base asphalt, the saturated components and aromatic phenols in the asphalt can be absorbed, thereby improving the low-temperature performance of the asphalt.

[0018] Optionally, the method for preparing the binder comprises the following steps:

[0019] Step S11: heating the base asphalt to 165±5° C., adding a chemical modifier, stirring for 20-30 minutes, and reacting sufficiently to obtain modified asphalt A;

[0020] Step S12: maintaining the temperature of the modified asphalt A, adding a polymer modifier, high-speed shearing for 20 to 35 minutes, a shear rate of 5000-7000 r / min, maintaining the temperature and stirring for 1-2 hours, to obtain modified asphalt B;

[0021] Step S13: Raise the temperature of the modified asphalt B to 180±5°C, add rubber powder, stir for 1-2h, then add the reinforcing agent, continue stirring for 30-60min, and cool to room temperature to obtain the binder.

[0022] In a second aspect, the present application provides a construction method for construction materials for seamless expansion joints of bridges and tunnels, which adopts the following technical solution:

[0023] A construction method for construction materials for seamless expansion joints of bridges and tunnels, comprising the following steps:

[0024] Step S21: slotting the seamless expansion joint of the pre-installed bridge and tunnel, and cleaning the inside of the slot;

[0025] Step S22: using primer to paint all the wall surfaces in the tank;

[0026] Step S23: heating the binder to 193° C. to 204° C., mixing it with the stone and stirring it evenly to obtain a mixture;

[0027] Step S24: Pave the mixture into the trough, and finally the upper surface of the construction exceeds the surrounding road surface by 8-10mm, and wait until the temperature drops below 40°C.

[0028] The present application distributes the enhancer and the synergist in two independent materials, and the two come into contact only when used, thus avoiding material failure caused by premature reaction between the two during storage.

[0029] By heating the binder during the construction process, not only can the binder be evenly mixed with the SBG-type stone that bears the skeleton structure, but the rate of the curing reaction is also greatly improved.

[0030] Due to thermal expansion and contraction, the top layer must exceed the height of the surrounding road surface when in a high temperature state to ensure that it can be flush with the surrounding road surface after cooling.

[0031] Optionally, the amount of primer used in step S22 is 1.5-3.0 kg / m 2 .

[0032] Normally, the preferred amount of primer is 1.8 kg / m 2 The dosage will be slightly adjusted with the surface roughness and structure depth, but will not exceed 1.5-3.0 kg / m 2 range.

[0033] Optionally, the mass ratio of the binder to the stone is 5-9:50.

[0034] Optionally, the stone is basalt or diorite, and when the stone passes through sieve holes with apertures of 20, 16, 12.5, and 4.75 mm, the corresponding passing ratios are 100%, 40%-100%, 15%-40%, and 0-20%, respectively.

[0035] Optionally, the mixed material in step S24 is paved into the trough body in a layer-by-layer manner for multiple times, with a construction thickness of 4-5 cm each time, and each layer of paving material must be cooled to below 40° C. before the next layer can be paved.

[0036] By adopting a multi-layer paving method, the construction quality can be ensured. The next layer can be paved after it is completely cooled and formed. This not only ensures a smoother paving, but also makes it easier to control the height difference caused by the final thermal expansion and contraction.

[0037] In summary, the present application includes at least one of the following beneficial effects:

[0038] 1. The present application distributes the enhancer and the synergist in two independent materials, and the two come into contact only when used, thereby avoiding premature reaction of the two during storage and causing material failure;

[0039] 2. The construction method provided in the present application, by heating the binder, can not only mix it evenly with the SBG-type stone, but also greatly increase the reaction rate of the reinforcing agent and the synergist. DETAILED DESCRIPTION

[0040] The present application provides a construction material for seamless expansion joints of bridges and tunnels, including a binder and a primer. The binder includes the following raw materials in parts by weight: 100 parts of base asphalt, 0.5-1 parts of chemical modifier, 3-5 parts of polymer modifier, 25-40 parts of rubber powder, and 5-15 parts of reinforcing agent; the chemical modifier can be preferably one or more of phosphoric acid, pyrophosphoric acid, and polyphosphoric acid; the polymer modifier can be preferably one or two of styrene-isoprene block copolymer and styrene-butadiene block copolymer.

[0041] The primer is composed of 801 glue and synergist, and the mass ratio of 801 glue to synergist is 10:1-3;

[0042] The mass ratio of synergist to enhancer is 1:5.

[0043] The preparation method of the above-mentioned binder comprises the following steps:

[0044] Step S11: heating the base asphalt to 160-170° C., preferably 165° C., adding a chemical modifier, stirring for 20-30 minutes, and reacting sufficiently to obtain modified asphalt A;

[0045] Step S12: maintaining the temperature of modified asphalt A, adding a polymer modifier, high-speed shearing for 20 to 35 minutes, a shear rate of 5000-7000 r / min, preferably 6000 r / min, maintaining the temperature and stirring for 1-2 hours, to obtain modified asphalt B;

[0046] Step S13: Raise the temperature of modified asphalt B to 175-185°C, preferably 180°C, add rubber powder, stir for 1-2h, then add reinforcing agent, continue stirring for 30-60min, cool to room temperature, and obtain the binder.

[0047] The present application also provides a construction method for construction materials for bridge and tunnel seamless expansion joints, comprising the following steps:

[0048] Step S21: slotting the seamless expansion joint of the pre-installed bridge and tunnel, and cleaning the inside of the slot;

[0049] Step S22: Use primer to paint all the wall surfaces of the tank body; the amount of primer used in step S22 can be 1.5-3.0 kg / m 2 , preferably 1.8 kg / m 2 ;

[0050] Step S23: heating the binder to 193°C to 204°C, preferably 200°C, and then mixing it with the stone and stirring it evenly to obtain a mixture; the mass ratio of the binder to the stone can be preferably 5-9:50; wherein the stone can be SBG type stone, specifically basalt or diorite, and when the SBG type stone passes through sieve holes with apertures of 20, 16, 12.5, and 4.75 mm, the corresponding passing ratios are 100%, 40%-100%, 15%-40%, and 0-20%, respectively;

[0051] Step S24: Pave the mixture layer by layer into the trough in multiple times, with a construction thickness of 4-5 cm each time. After each layer of paving material cools to below 40°C, pave the next layer, and the top layer protrudes 8-10mm beyond the surrounding road surface. Wait until the temperature drops below 40°C.

[0052] The solution of the present application will be further described below through specific embodiments. It should be noted that the size of the troughs used for paving construction materials in the following embodiments and comparative examples is consistent.

[0053] Example 1

[0054] Example 1 provides a construction material for seamless expansion joints of bridges and tunnels, which includes a binder and a primer.

[0055] ① The amount of binder is shown in Table 1. The preparation method is carried out according to the following steps:

[0056] Step S11: heating the base asphalt to 165° C., adding a chemical modifier, stirring for 20 minutes, and reacting sufficiently to obtain modified asphalt A;

[0057] Step S12: maintaining the temperature of the modified asphalt A, adding a polymer modifier, high-speed shearing for 30 minutes, a shear rate of 6000 r / min, maintaining the temperature and stirring for 1 hour, to obtain modified asphalt B;

[0058] Step S13: Raise the temperature of modified asphalt B to 180°C, add rubber powder, stir for 1 hour, then add reinforcing agent, continue stirring for 60 minutes, and cool to room temperature.

[0059] Among them, the reinforcing agent is E41 epoxy resin.

[0060] ② The amount of primer is as shown in Table 1, and the preparation method is carried out according to the following steps:

[0061] Just mix 801 glue and the synergist evenly; the synergist is specifically ultra-fine powdered dicyandiamide, and its average particle size is 5-10μm.

[0062] Table 1 Amounts of binder raw materials and primer raw materials used in each example

[0063]

[0064] Example 2-3

[0065] Example 2-3 provides a construction method for construction materials for seamless expansion joints of bridges and tunnels, which is basically the same as Example 1, with the only difference being the different amounts of raw materials used in the binder and primer, as shown in Table 1 for details.

[0066] Comparative Example 1

[0067] Comparative Example 1 is substantially the same as Example 1, except that the amount of the synergist used in the primer of Comparative Example 1 is 0.05 kg.

[0068] Comparative Example 2

[0069] Comparative Example 2 is substantially the same as Example 1, except that no synergist is added to the primer of Comparative Example 2.

[0070] Comparative Example 3

[0071] Comparative Example 3 is basically the same as Example 1, except that the amount of reinforcing agent in the binder of Comparative Example 3 is 0.25 kg.

[0072] Comparative Example 4

[0073] Comparative Example 4 is basically the same as Example 1, except that no reinforcing agent is added to the binder of Comparative Example 4.

[0074] Comparative Example 5

[0075] Comparative Example 5 is substantially the same as Example 1, except that the primer is missing in Comparative Example 5.

[0076] The direction of the road wheel load is perpendicular to the road surface and parallel to the contact surface between the product of the present invention and the tank body, so in actual use, the destructive stress borne by the present invention is shear stress. Therefore, we tested the tensile shear strength of the construction materials prepared in the above Examples 1-3 and Comparative Examples 1-5, and the specific test method is as follows:

[0077] 1) Specimen preparation. The shape and size of the specimens refer to the requirements of Section 5.1 of GB / T 7124-2008 Determination of tensile shear strength of adhesives. Prepare two specimens for each test. First, apply the primer evenly on the bonding surface of one specimen, and then apply the binder on the bonding surface of the other specimen. Apply a thin layer. Then, stick the bonding surfaces of the two specimens together and keep them in an oven at 160-170°C for more than 30 minutes to allow them to react fully, and then cool them to room temperature.

[0078] 2) Specimen testing. The specimen that has been cooled to room temperature is clamped on the fixture, with the distance from the clamp to the nearest bonding end being 50mm±1mm. A tensile test is performed using a tensile testing machine at a constant test speed of 50mm / min, with the tensile direction parallel to the bonding surface of the specimen. The maximum load of the specimen shear failure is recorded as the failure load, and the shear strength of the specimen is calculated in combination with the bonding area of ​​the specimen.

[0079] Table 2 Test results of Examples 1-3 and Comparative Examples 1-5

[0080] Example No. Shear strength / Mpa Comparative Example No. Shear strength / Mpa Example 1 8.1 Comparative Example 1 3.7 Example 2 8.8 Comparative Example 2 2.0 Example 3 8.3 Comparative Example 3 4.5 / / Comparative Example 4 2.6 / / Comparative Example 5 0.6

[0081] It can be seen from the results in Table 2 that the construction materials prepared in Examples 1-3 all have good shear strength. Compared with Example 1, Comparative Examples 1 and 2 have no synergist or too little synergist in the primer, which will result in too low shear strength of the construction materials, and thus fail to meet the construction requirements of seamless expansion joints of bridges and tunnels. Compared with Example 1, Comparative Examples 3 and 4 have no reinforcing agent or too little reinforcing agent in the binder, which will also result in too low shear strength of the construction materials, and fail to meet the construction requirements of seamless expansion joints of bridges and tunnels. Compared with Example 1, since the bonding surface area of ​​one of the test pieces lacks primer, in the case of only binder, the shear strength of the construction material obtained is lower than that of Comparative Examples 1-2, indicating that only when the binder is used in combination with the primer, and the reinforcing agent and synergist therein can meet a certain ratio, can the shear strength of the construction material reach a higher level.

[0082] The present application further verifies the feasibility of the construction materials prepared in the above Examples 1-3 in practical applications, and applies them to the construction of seamless expansion joints of bridges and tunnels, thus providing Application Examples 1-3.

[0083] Application Example 1

[0084] The ingredients are prepared according to the proportion of each raw material used in Example 1 in Table 1, and the binder is used in combination with the stone to provide a skeleton support for the expansion joint. It should be noted that Example 1 only gives the amount of each raw material used on a laboratory scale. In actual applications, the amount of each raw material used far exceeds the actual amount given in Example 1, and is specifically controlled by increasing the amount used in Example 1 in equal proportion.

[0085] The stone used in the construction is SBG type stone, specifically basalt, which has a passing ratio of 100%, 40%, 15%, and 0% when passing through sieve holes with apertures of 20, 16, 12.5, and 4.75 mm, respectively; the mass ratio of binder to stone is 1:10. The specific construction steps are as follows:

[0086] Step S21: slotting the seamless expansion joint of the pre-installed bridge and tunnel, and cleaning the inside of the slot;

[0087] Step S22: Use the primer of Example 1 to paint all the wall surfaces of the tank; the amount of primer used is 1.8 kg / m 2 ;

[0088] Step S23: heating the binder of Example 1 to 200° C., mixing it with the stone and stirring it evenly to obtain a mixture;

[0089] Step S24: Pave the mixture layer by layer into the trough in multiple times, with a construction thickness of 5 cm each time. After each layer of paving material cools to below 40°C, pave the next layer, and the top layer protrudes 10mm beyond the surrounding road surface. Wait until the temperature drops below 40°C.

[0090] Application Example 2

[0091] Application Example 2 is basically the same as Application Example 1, the only difference being that the construction materials (i.e., primer and binder) used in the construction process are in the same proportion as those in Example 2.

[0092] Application Example 3

[0093] Application Example 3 is basically the same as Application Example 1, the only difference being that the construction materials (i.e., primer and binder) used in the construction process are in the same proportion as those in Example 3.

[0094] According to the Test Code for Asphalt and Asphalt Mixtures in Highway Engineering (JTJ E20-2011), the high temperature stability and low temperature crack resistance of the seamless expansion joints of the bridges and tunnels constructed in Examples 1-3 were tested.

[0095] The tensile strength test was carried out on the seamless expansion joints of the bridge and tunnel constructed in the corresponding use cases 1-3 according to GB / T 6329.

[0096] Table 3 Test results of various application examples

[0097] Test items Dynamic stability at 60℃ / times / mm Maximum bending strain at -10℃ / με Tensile strength (23℃) / Mpa Technical requirements >6000 >2800 >1.1 Application Example 1 8044 3342 1.2 Application Example 2 8453 3781 1.4 Application Example 3 8235 3526 1.3

[0098] It can be seen from the results in Table 3 that the results obtained in Application Examples 1-3 all meet the technical requirements, especially the high temperature stability and low temperature crack resistance, the results of which greatly exceed the lower limit of the technical requirements, indicating that the construction materials prepared according to the raw material formula of Examples 1-3 can meet the construction requirements of seamless expansion joints of bridges and tunnels. According to this application, the stability and durability of seamless expansion joints under high traffic flow will be greatly improved.

[0099] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A construction material for seamless expansion joints of bridges and tunnels, characterized in that: It comprises a binder and a primer, wherein the binder comprises the following raw materials in parts by weight: 100 parts of base asphalt, 0.5-1 parts of chemical modifier, 3-5 parts of polymer modifier, 25-40 parts of rubber powder, and 5-15 parts of reinforcing agent; The primer is composed of 801 glue and a synergist, and the mass ratio of the 801 glue to the synergist is 10:1-3; The mass ratio of the synergist to the enhancer is 1:5; The chemical modifier is one or more of phosphoric acid, pyrophosphoric acid, and polyphosphoric acid; The polymer modifier is one or both of styrene-isoprene block copolymer and styrene-butadiene block copolymer; The reinforcing agent is E41 type epoxy resin, and the synergist is ultra-fine powdered dicyandiamide.

2. The construction material for seamless expansion joints of bridges and tunnels according to claim 1, characterized in that: The preparation method of the binder comprises the following steps: Step S11: heating the base asphalt to 165±5° C., adding a chemical modifier, stirring for 20-30 minutes, and reacting sufficiently to obtain modified asphalt A; Step S12: maintaining the temperature of the modified asphalt A, adding a polymer modifier, high-speed shearing for 20 to 35 minutes, a shear rate of 5000-7000 r / min, maintaining the temperature and stirring for 1-2 hours, to obtain modified asphalt B; Step S13: Raise the temperature of the modified asphalt B to 180±5°C, add rubber powder, stir for 1-2h, then add the reinforcing agent, continue stirring for 30-60min, and cool to room temperature to obtain the binder.

3. The construction method of the construction material for bridge and tunnel seamless expansion joint according to claim 1 or 2, characterized in that: The steps include: Step S21: slotting the seamless expansion joint of the pre-installed bridge and tunnel, and cleaning the inside of the slot; Step S22: using primer to paint all the wall surfaces in the tank; Step S23: heating the binder to 193° C. to 204° C., mixing it with the stone and stirring it evenly to obtain a mixture; Step S24: Pave the mixture into the trough, and finally the upper surface of the construction exceeds the surrounding road surface by 8-10 mm, and wait until the temperature drops below 40°C.

4. The construction method of the construction material for seamless expansion joints of bridges and tunnels according to claim 3 is characterized in that: The amount of primer used in step S22 is 1.5-3.0 kg / m 2 .

5. The construction material for seamless expansion joints of bridges and tunnels according to claim 3, characterized in that: The mass ratio of the binder to the stone is 5-9:

50.

6. The construction material for seamless expansion joints of bridges and tunnels according to claim 3, characterized in that: The stone is basalt or diorite, and when the stone passes through sieve holes with apertures of 20, 16, 12.5, and 4.75 mm, the corresponding passing ratios are 100%, 40%-100%, 15%-40%, and 0-20%, respectively.

7. The construction method of the construction material for seamless expansion joints of bridges and tunnels according to claim 3, characterized in that: The mixed material in step S24 is paved into the tank body in layers for multiple times, with each layer of paving material being 4-5 cm thick, and each layer of paving material must be cooled to below 40° C. before the next layer can be paved.

Citation Information

Patent Citations

  • Material for waterproof bridge surface system and its paving process

    CN101021058A

  • Epoxy asphalt bonding layer material for cement concrete bridge surface and preparation method thereof

    CN102757761A

  • Quick patching material for expansion joint and preparation method thereof

    CN103964748A

  • Application of a random-laid web for roadway construction with improved adhesion properties

    CN106436520A

  • High-viscosity high-elasticity asphalt for seamless expansion joint and preparation method of high-viscosity high-elasticity asphalt

    CN108659555A