A high carbon cold heading steel wire rod for 14.9 grade non-quenched and tempered bolts and a manufacturing method thereof
Through the design of high-carbon carbon components and online molten salt phase change control technology, a suitable microstructure structure is formed, which solves the problem of difficulty in taking into account the strength and plasticity of the 14.9-level cold heading steel strips, and realizes an efficient and low-cost manufacturing process , simplifies the process and improves the yield rate.
Patent Information
- Application Number
- CN202411125828.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The prior art is difficult to develop high-strength and high-plastic cold-headed steel strips for 14.9-grade non-temperature bolts without increasing material costs. The existing process is complex and the production efficiency is low, which can easily lead to brittle breakage and Waste of materials.
Designed with high-carbon carbon components, the chemical components include C: 0.79%~0.83%, Si: 0.15%~0.25%, Mn: 0.58%~0.72%. Through the online molten salt phase change regulation technology, tempered pearlite is formed. The mixed structure of tempered scornithite and tempered bainite is combined with the roller slow cooling process to regulate the microstructure structure of the strip.
The matching of high strength and high plasticity is achieved, the cost of materials is reduced, the manufacturing process is simplified, the manufacturing process is avoided, the material waste is increased, and the material yield is improved, and it is suitable for efficient green manufacturing under non-temperature processes.
Smart Images

Figure CN118639120B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cold heading steel wire rods, and in particular relates to a high carbon cold heading steel wire rod for 14.9 grade non-quenched and tempered bolts and a manufacturing method thereof. Background Art
[0002] Bolt connection is an important connection method and is widely used in machinery, automobiles, construction and other fields. With the development trend of lightweight structural steel, the strength grade of steel is constantly improving, and the service stress conditions of bolts as connecting components are also constantly improving. Therefore, the strength grade of bolts needs to be continuously improved to meet the growing application of high-stress industrial fields. Cold heading steel wire rods for bolts are used as base materials, which plays a vital role in improving the strength grade of bolts. Therefore, the strength grade of cold heading steel wire rods is required to be continuously improved. However, there are many studies on the manufacturing of 8.8~12.9 grade bolts and their cold heading steel wire rods in the prior art. Due to the difficulty in developing bolts with higher performance grades of 13.9 and above, such as 14.9 grade bolts with tensile strength requirements of >1400MPa and high-speed wire cold heading steel, the strength grade of the component system is mainly guaranteed by increasing the content of hardenability alloying elements on the basis of low and medium carbon and adding a variety of micro-alloying elements, but at the same time it brings a significant increase in material costs, which is affected by the hot rolling of wire rods. Due to the influence of the cooling rate of the subsequent Stelmor air-cooled line, the high hardenability of the composition system will aggravate the risk of precipitation of abnormal structures such as martensite and bainite that deteriorate the drawing performance, resulting in brittle fracture and difficulty in coiling of the finished product, and a low yield. Therefore, cold heading steel will be developed in the form of round steel to adapt to mass production. For example, patent CN110106443A discloses a method for producing round steel for ultra-high strength bolts, which takes 42CrMo as the base material and is developed into 14.9-grade cold heading steel through complex processes such as rolling, blanking, slow cooling, and heat treatment. Although it avoids the problem of high-line coiling, it is difficult to directly obtain small-sized raw materials, the process is complicated, the production efficiency is low, and the production cost is high.
[0003] For example, patent CN118186298A discloses a high-plasticity delayed fracture resistant ultra-high-strength fastener steel wire rod and its manufacturing method, which adopts a medium C-Si-Mn-Cr-Mo-V-Al-Ni composition design, and after spinning, air cooling on the Stelmor air cooling line and then insulation and slow cooling to obtain a hot-rolled metallographic structure mainly composed of bainite and a small amount of martensite and ferrite, and can obtain a lower bainite structure through molten salt isothermal heat treatment to achieve 14.9 grade fastener mechanical properties, but on the one hand, the high Cr content and the addition of expensive components such as Mo, V, and Ni also make the steel material cost higher. In order to reduce costs, alloy elements or Reducing the alloy content will lead to a significant loss of wire rod strength and hardenability. Bainite and martensite, as hard and brittle phase structures with high distortion and dislocation density, are difficult to soften during the continuous cooling process of insulation treatment on the Stelmor air cooling line, causing the wire rod to break brittlely during coiling at the steel plant, transportation to downstream users and uncoiling by downstream users, resulting in material waste, reduced yield and increased fastener manufacturing costs. On the other hand, although salt bath treatment is adopted, it is an offline salt bath. Downstream users need to unpack the coils, uncoil them, heat them to the austenitizing temperature and conduct long-term molten salt treatment, resulting in increased procedures, energy consumption and costs, which is not conducive to the efficient production of fasteners.
[0004] The existing cold heading steel wire rod for bolts of grade 12.9 and below still needs to undergo multiple spheroidizing annealing, drawing, cold heading and tempering processes to manufacture bolts. Spheroidizing annealing is used to improve the cold deformation performance. After drawing and cold heading to reduce the surface and increase the strength, tempering is required to further improve the comprehensive mechanical properties to achieve the final performance level. For cold heading steel wire rod for bolts of grade 14.9, it is even more necessary to develop non-tempered cold heading steel wire rod for bolts that can save the spheroidizing annealing and tempering processes, so as to simplify bolt manufacturing, reduce emissions and energy consumption, and realize its efficient and green manufacturing. However, the higher strength grade of the cold heading steel wire rod also brings challenges to the improvement of the plasticity of the wire rod.
[0005] High carbon steel uses carbon to replace other alloying elements, which has the advantage of lower material cost. However, the existing high carbon steel wire rods mainly focus on increasing the troostite content in the structure to achieve the improvement of the strength grade of bridge cables, cords, etc. and obtain appropriate drawing performance. It is difficult to apply it to cold heading steel wire rods. The reasons include: First, the Stelmor air-cooled line adopts insulation or delayed cooling to reduce the risk of abnormal structure and promote the incubation of troostite, but the time in the precipitation temperature range of secondary cementite is relatively long. High carbon elements will cause the wire rod to form a network carbide deterioration phase during the cooling process of the air-cooled line, which will destroy the continuity of the structure, especially increase the brittleness of the material, and it is difficult to eliminate it by annealing or tempering, which is more likely to cause cracking during drawing and cold heading under non-tempering processes; Second, due to the small degree of supercooling and the short time the wire rod passes through the troostite phase area under continuous insulation cooling, The wire rod after being inoculated with troostite is already in a low-temperature state, so the interlamellar spacing of the obtained troostite structure is large, and the structural stress and dislocation density are high, which makes the wire rod ultimately insufficient in plasticity, poor in cold deformation ability, and easy to be hardened by drawing, and cannot meet the requirements of drawing and cold heading. Increasing the ferrite content in the structure will cause a significant deterioration in the strength of the wire rod, which is not conducive to the performance level of 14.9 bolts without quenching and tempering. Third, the increase in carbon content makes the lamella thicker, and the increase in alloying elements slows down the diffusion of carbon. Although the hardenability of the wire rod can be used to appropriately increase the cooling rate and form a certain amount of bainite by phase transformation, bainite as a low-temperature structure will also be because the wire rod has dropped to a low-temperature state during the continuous cooling phase transformation process, and cannot be softened, which significantly increases brittleness. It is impossible to directly obtain a high-strength, high-plasticity wire rod, resulting in a loss of yield and the risk of cracking in non-quenching and tempering processes. Summary of the invention
[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a high-carbon carbon cold heading steel wire rod for 14.9-grade non-quenched and tempered bolts and a manufacturing method thereof, which can effectively reduce material costs by utilizing high-carbon carbon components, realize wire rod microstructure regulation, and match high strength with high plasticity, and is used for efficient and green manufacturing of 14.9-grade bolts under non-quenched and tempered processes, effectively reducing the risk of cracking and improving the yield rate.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] A high-carbon carbon cold-heading steel wire rod for 14.9-grade non-quenched and tempered bolts, the chemical composition and mass percentage of the cold-heading steel wire rod include: C: 0.79%-0.83%, Si: 0.15%-0.25%, Mn: 0.58%-0.72%, P≤0.015%, S≤0.015%, and the rest is Fe and unavoidable impurities; its microstructure includes 50%-60% by volume of tempered pearlite, 5%-10% by volume of tempered bainite, 25%-35% by volume of tempered troostite, and the rest is a mixed structure composed of fused pearlite.
[0009] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:
[0010] (1) Carbon: As the main added element, C is cheaper than other alloying elements. It is used to ensure the matrix strength, high hardenability and wear resistance of steel through solid solution strengthening, so that the performance level of 14.9 bolts can be achieved through drawing and cold heading after omitting annealing and tempering processes. However, it also increases the risk of decarburization of steel, the risk of cementite distribution along grain boundaries and aging sensitivity. If the C content is too high, the cementite lamellae will become thicker and the diffusion of carbon will slow down, which is not conducive to the melting and softening of the organization regulated by the online molten salt phase transformation. Therefore, in order to facilitate organization regulation and take into account the cold deformation performance and strength characteristics of cold heading steel wire rod, the mass percentage of C is controlled to be 0.79%~0.83%.
[0011] (2) Silicon: The Si element is a deoxidizer in the steelmaking process. It can dissolve in austenite to increase the hardness and strength of steel. It can inhibit the grain coarsening of the first stage of molten salt treatment in the online molten salt phase transformation regulation, which is beneficial to the nucleation of bainite and troostite. However, excessive silicon will increase the risk of non-metallic inclusions and decarburization, increase the degree of cold work hardening of steel, and reduce the cold plastic deformation and toughness of steel. Therefore, the mass percentage of Si is controlled to be 0.15%~0.25%.
[0012] (3) Manganese: Mn is often added to steel as a deoxidizer and desulfurizer during the smelting process. It can be infinitely dissolved in Fe and dissolved in austenite to improve the strength level, hardenability and wear resistance of steel. It also increases the degree of supercooling during austenite cooling, which is beneficial for the wire rod to quickly transform into bainite and troostite with finer interlamellar spacing after passing through the first molten salt. However, too high a Mn content will aggravate the segregation during the solidification of the billet, resulting in poor uniformity of the steel, increase the tendency of grain coarsening during the heating process of the material, affect the activity of C and increase the difficulty of tempering softening. Therefore, the mass percentage of Mn is controlled to be 0.58%~0.72%.
[0013] (4) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.
[0014] The cold heading steel wire rod is designed with a high carbon component of high C-Si-Mn, and uses low-cost C as the main component to replace the addition of alloy components such as Cr, Mo, Ti, V, Nb, B, and Ni, which can effectively reduce material costs and ensure matrix strength and high hardenability. The cold heading steel wire rod structure includes most tempered pearlite, a small part of tempered bainite, a small amount of tempered bainite and fused pearlite. The interlamellar spacing of pearlite is larger than that of bainite, the plasticity is better than that of bainite, and the strength is higher than that of ferrite. The tempered pearlite retains the characteristics of moderate strength and plasticity of pearlite, and the melting and hardening of pearlite are not bad. After the spheroidized structure is transformed into fused pearlite and tempered pearlite, the organizational stress and dislocation density are further reduced, and the plastic properties are improved. The interlamellar spacing of troostite is smaller than that of pearlite, the strength is higher than that of pearlite, and it has better drawing properties. After the spheroidized structure of troostite is transformed into tempered troostite, the dislocation density is further reduced, which can provide a certain matrix strength and effectively reduce drawing hardening. Tempered bainite retains the characteristic that bainite has higher strength than soft phase structures such as pearlite and ferrite. After bainite is transformed into tempered bainite through tempering, the dislocation density is further reduced, which significantly improves the plasticity.
[0015] Therefore, compared with the existing hot-rolled medium- and low-carbon alloy cold heading steel wire rod structure containing bainite or mainly bainite, the cold heading steel wire rod can provide higher matrix strength through high carbon components combined with tempered bainite and tempered troostite, making up for the strength loss caused by eliminating alloy elements and reducing alloy content, and can effectively and significantly improve the plasticity of the wire rod by regulating the tempered structure of pearlite, bainite and troostite, making up for the adverse effects of high carbon components and bainite hard and brittle phase structure on cold deformation performance. Compared with the existing high-carbon steel wire rod with high troostitization rate, the cold heading steel wire rod can also effectively improve the organizational stress and troostite dislocation density by appropriately adding tempered pearlite and fused pearlite structure, which can effectively reduce pull hardening and cold heading cracking, thereby achieving high strength and high plasticity matching of high carbon carbon components, and is suitable for the manufacture of 14.9 grade non-quenched and tempered bolts.
[0016] In a preferred embodiment, the interlamellar spacing of the tempered pearlite is 155~185nm, and the interlamellar spacing of the tempered bainite is 75~105nm. The decrease in the interlamellar spacing of the tempered bainite is accompanied by an increase in the proportion of tempered bainite, an increase in the strength of the wire rod and a decrease in the plasticity. The increase in the interlamellar spacing of the tempered pearlite is accompanied by an increase in the proportion of fused pearlite, a decrease in the strength of the wire rod and an increase in the plasticity.
[0017] In a preferred embodiment, the network carbide level of the cold heading steel wire rod is level 0, which can effectively inhibit the formation of network carbides, avoid the risk of cracking caused by them, and enhance the economic value of carbon elements.
[0018] In a preferred embodiment, the diameter of the cold heading steel wire rod is 5.5~12.0mm, the tensile strength is 1305~1345MPa, and the cross-sectional shrinkage rate is 44%~49%. It has a smaller diameter specification than the existing 14.9 grade cold heading round steel for bolts, which is conducive to simplifying and reducing the manufacturing difficulty of small-size bolts. Compared with the existing low-grade or quenched and tempered cold heading steel wire rods for fasteners, the cold heading steel wire rod has significantly improved tensile strength and cross-sectional shrinkage rate. Compared with the existing bainite structure wire rod, it can effectively avoid brittle fracture during winding, transportation and downstream unwinding, and reduce raw materials. Waste is reduced and the yield rate is improved. After the annealing process is omitted, the tensile strength and forming of the wire rod can be further improved by drawing and cold heading. The performance grade of 14.9 can be achieved through simple aging treatment without the quenching and tempering process. Due to the high plasticity of the wire rod, it is not easy to crack during the cold working process without the annealing and tempering processes. Due to the high strength of the wire rod, it can be strengthened to the performance grade of 14.9 through simple drawing and cold heading. The process will not cause excessive loss of plasticity of the wire rod, thereby reducing the risk of wire breakage and cracking, simplifying the bolt manufacturing process and reducing the overall cost.
[0019] A method for manufacturing a 14.9-grade non-quenched and tempered high-carbon carbon cold-heading steel wire rod for bolts, the manufacturing method comprising: producing a wire rod by controlled rolling according to the chemical composition of the 14.9-grade non-quenched and tempered high-carbon carbon cold-heading steel wire rod for bolts described in any one of the above items, after the wire rod is spun into a wire rod at a spinning temperature of ≥935°C, an online molten salt phase transformation control is performed, the wire rod first passes through a first section of molten salt, the wire rod is cooled at a cooling rate of ≥44°C / s to a bainite and troostite phase region for a structural phase transformation, and a part of austenite is promoted to bainite. The wire rod is then heated to the isothermal state in the pearlite phase region through the final molten salt to promote the transformation of untransformed austenite to pearlite, and at the same time promote the tempering and softening of bainite, bainite and pearlite. Finally, it is slowly cooled through a roller to form a cold heading steel wire rod with a microstructure including 50% to 60% tempered pearlite by volume, 5% to 10% tempered bainite by volume, 25% to 35% tempered bainite by volume, and the rest is a mixed structure composed of fused pearlite.
[0020] Compared with the existing limitations that the spinning temperature of high carbon steel wire rod cannot be too high in order to reduce the risk of abnormal tissue precipitation or to prolong the incubation of troostite phase transformation but the online time should not be too long, the above-mentioned manufacturing method adopts online molten salt phase transformation regulation directly after spinning, which can quickly cool down and regulate the structure, so it can break the low-temperature spinning limitation and select a higher spinning temperature. On the one hand, it is used to avoid the formation of secondary cementite precipitation in the spinning stage and inhibit the network carbide. On the other hand, it provides favorable conditions for the subsequent formation of a higher degree of supercooling through the first stage of molten salt and promotes the troostite phase transformation with finer interlamellar spacing.
[0021] When the wire rod after spinning is subjected to online molten salt phase transformation control, it first passes through the first section of molten salt. Compared with the maximum cooling rate of the Stelmore air-cooling line, which can only reach about 10°C / s, the high heat exchange capacity of the molten salt can be used to cool the wire rod extremely quickly. On the one hand, it can pass through the secondary network carbon precipitation interval at an ultra-fast cooling rate to inhibit the formation of network carbides and effectively improve the economic value of the carbon element. On the other hand, it can form a large degree of supercooling to inhibit the precipitation of proeutectoid ferrite, so that the wire rod can quickly enter the bainite and troostite phase region for organizational phase transformation. Through a lower isothermal temperature and a short isothermal phase transformation, part of the high-temperature austenite is promoted to transform into bainite and troostite with fine interlamellar spacing, so as to control the content of tempered bainite and tempered troostite. At the same time, compared with the strong wind cooling environment, since the molten salt can cover the surface of the wire rod when the wire rod passes through the molten salt, there is no temperature difference problem between the windward side and the leeward side, which can avoid the occurrence of abnormal martensitic organization in the wire rod and reduce the fluctuation of the mechanical properties of the wire rod.
[0022] The wire rod that has passed through the first stage of molten salt and then the final stage of molten salt with increased temperature can quickly reach the pearlite phase transformation temperature range, thereby promoting the transformation of the untransformed high-temperature austenite in the wire rod to pearlite structure after passing through the first stage of molten salt. At the same time, compared with the existing continuous cooling phase transformation control process of heat preservation and slow cooling, the above-mentioned manufacturing method can also utilize the terminal molten salt to increase the temperature after the organizational phase transformation, and the wire rod and the molten salt temperature are consistent, thereby extending the time of the wire rod in the high temperature range, and promoting the tempering and softening of bainite, troostite and pearlite structures after the phase transformation, thereby continuously reducing the matrix dislocation density and adjusting the carbide morphology, thereby regulating the matrix strength and plasticity. It also avoids the occurrence of abnormal martensitic structure in the subsequent cooling process of the wire rod. After slow cooling on the roller, the high temperature state of the wire rod after passing through the molten salt can be used to promote the one-step softening of the tempered bainite, troostite and pearlite structures, so as to achieve the final structure control and strength-plastic performance matching. Compared with the offline salt bath process, this online molten salt phase change control of direct salt bath after spinning can not only solve the difficulties of abnormal structure and strength-plastic performance control of the existing Stelmor line controlled cooling, avoid brittle fracture and yield rate problems, but also avoid the adverse effects on efficiency and cost of reheating and heat treatment of wire rod by downstream users.
[0023] In a preferred embodiment, during the controlled rolling, the heating furnace temperature is controlled to be 1050~1100°C before rolling, the furnace time is 2~4h, the oxygen content in the furnace is ≤1.4%, and a lower heating furnace temperature and a shorter furnace time are selected to promote uniform diffusion of components and combine with low furnace oxygen content to inhibit high-temperature oxidation and control the degree of decarburization of high-carbon steel billets.
[0024] By adopting a higher spinning temperature, the limitation of low-temperature spinning on low-temperature rolling can be broken, and a higher rolling temperature is selected to reduce the wear on the rolling line and increase the rolling speed. In a preferred embodiment, during the controlled rolling, the initial rolling temperature is controlled to be 1030~1075℃, and the initial rolling reduction is 20%~28%. The higher initial rolling temperature is selected to promote composition homogenization, and the austenite grains are refined through repeated deformation and recrystallization.
[0025] In a preferred embodiment, during the controlled rolling, the final rolling temperature is controlled to be ≥950°C, and the final rolling reduction is 32%~42%. Selecting a higher final rolling temperature is beneficial to the dissolution of carbides in high carbon steel and increases the stability of austenite. Selecting a larger final rolling reduction reduces the tendency of austenite grain growth, creating favorable conditions for refining the structure and controlling the network carbides.
[0026] In a preferred embodiment, the molten salt temperature of the first stage molten salt is 420~450℃, and the processing time is 5~15s. The lower the molten salt temperature of the first stage molten salt and the longer the processing time, the more austenite transforms to bainite, the finer the troostite lamellae spacing, the higher the proportion of tempered bainite, the higher the strength of the wire rod and the lower the plasticity. However, if the molten salt temperature of the first stage molten salt is too low, the proportion of tempered bainite is too high or the troostite structure cannot be obtained. If the processing time is too long, the more bainite and troostite transform, which is not conducive to the plasticity of the wire rod. On the contrary, the higher the molten salt temperature and the shorter the time, the smaller the proportion of tempered bainite, the larger the troostite lamellae spacing, the lower the strength of the wire rod and the higher the plasticity. However, if the molten salt temperature is too high and the time is too short, it is not conducive to the transformation of bainite, and even the troostite structure with finer lamellae cannot be obtained, which will result in a significant loss of matrix strength and excessive degradation of the strength of the wire rod.
[0027] In a preferred embodiment, the molten salt circulation rate of the first stage molten salt is 350~550t / h, and the molten salt temperature rise is ≤10°C. The molten salt circulation rate can be used to control the molten salt temperature rise to maintain the processing accuracy, avoid unnecessary energy consumption caused by excessive molten salt circulation rate, and avoid abnormal organization and regulation differences caused by too small molten salt circulation rate.
[0028] In a preferred embodiment, the molten salt temperature of the final molten salt is 460-520°C, and the processing time is 200-400s. The lower the molten salt temperature of the final molten salt, the finer the pearlite lamella spacing formed. The refined lamella spacing can reduce the difficulty of melting. However, if the molten salt temperature is too low, the proportion of troostite increases due to supercooling, which will affect the plasticity of the wire rod. On the contrary, the higher the molten salt temperature, the coarser the pearlite lamella spacing formed, which can provide more thermal power for the tempering and softening of bainite, troostite and pearlite structures, thereby reducing the strength of the wire rod and increasing the plasticity. However, if the molten salt temperature is too high, it is easy to cause the lamella to be too coarse or form a ferrite structure, which will cause excessive tempering and softening and will have a great impact on the wire rod. Strength is unfavorable; the longer the treatment time of the final molten salt, the more obvious the tempering softening effect of reducing the matrix dislocation density and adjusting the carbide morphology to spheroidization, the wire rod strength decreases and the plasticity increases, but if the treatment time is too long, excessive softening will cause a large strength loss, and it is not conducive to efficient production. On the contrary, the shorter the treatment time, the worse the tempering softening effect, the wire rod plasticity decreases, and even the treatment time is too short to affect the full incubation of pearlite and increase the risk of abnormal tissue precipitation, which is not conducive to tissue regulation. Therefore, the molten salt temperature and treatment time of the final molten salt can be further controlled to promote the transformation of untransformed high-temperature austenite to pearlite, and at the same time, tempering softening regulates matrix strength and plasticity.
[0029] In a preferred embodiment, the molten salt circulation rate of the final molten salt is 350~550t / h, and the molten salt temperature rise is ≤5°C. Selecting a higher molten salt circulation rate to control the molten salt temperature rise can promote uniform tissue transformation and tempering softening, and avoid unnecessary energy consumption increase caused by excessive molten salt circulation rate.
[0030] In a preferred embodiment, the roller slow cooling adopts closing the insulation cover, controlling the wire rod to be cooled to below 300°C at a cooling rate of 0.35~0.80°C / s, and forming an insulation channel structure by closing the insulation cover. The wire rod that has passed through the last section of molten salt is transported by rollers and continuously slowly cooled in the insulation cover. If necessary, the hot air generated during the online molten salt phase change regulation process can be input into the insulation cover to control the cooling rate of the wire rod. The slow cooling rate can be used to extend the time that the wire rod is at high temperature, promote further softening of the wire rod structure, and then coil it.
[0031] Compared with the prior art, the beneficial effects of the present invention are at least:
[0032] (1) In view of the current situation that the existing cold heading steel wire rod increases the content of hardenability alloying elements and adds a variety of microalloying elements to improve the system strength, but it brings high material cost, increased risk of abnormal structure precipitation and difficulty in balancing plasticity, the cold heading steel wire rod of the present invention adopts a high carbon carbon component design with high C-Si-Mn, which can save Cr, Mo, Ti, V, Nb, B, Ni and other alloy components, effectively reducing material costs. The microstructure includes most tempered pearlite, a small part of tempered bainite, a small amount of tempered bainite and fused pearlite, but does not include martensite structure. It can use high carbon solid solution strengthening combined with tempered bainite and tempered bainite structure to provide matrix strength, making up for the omission of alloy The strength loss caused by the composition can be combined with the tempering microstructure regulation of pearlite, bainite and troostite to effectively reduce the microstructure stress and dislocation density, significantly improve the plasticity of the wire rod, make up for the adverse effects of high carbon composition and bainite hard and brittle phase structure on cold deformation performance, reduce drawing hardening and cold upsetting cracking, achieve high strength and high plasticity matching, and achieve a tensile strength of 1305~1345MPa and a cross-sectional shrinkage rate of 44%~49%. It can avoid the brittle fracture problems of coiling, transportation and downstream unwinding and improve the yield rate, and can be suitable for the efficient and green manufacturing of 14.9 grade bolts under non-quenching and tempering process, reduce carbon emissions and bolt costs, and has good market application prospects.
[0033] (2) In view of the current situation that high-speed wire cold heading steel is affected by the cooling rate of the Stelmor air-cooled line, resulting in the development of cold heading steel in the form of round steel or it is difficult to meet the application requirements of 14.9 grade non-quenched and tempered bolts, the manufacturing method of the present invention combines the design of high carbon carbon components with the online molten salt phase change control technology, which can select a higher wire drawing temperature, combined with the subsequent online molten salt rapid cooling, and the first stage of molten salt passes through the secondary network carbon precipitation zone at an ultra-fast cooling rate, thereby inhibiting the formation of network carbides, effectively improving the economic value of carbon elements, and promoting the transformation of part of the high-temperature austenite to bainite and troostite structure, thereby further improving the economic value of carbon elements. The content of matrix tempered bainite and tempered troostite is effectively controlled to ensure matrix strength and plasticity, and then the final molten salt is used to promote the transformation of untransformed high-temperature austenite to pearlite. At the same time, the bainite, troostite and pearlite structures transformed from high-temperature austenite are tempered and softened, continuously reducing the matrix dislocation density and adjusting the carbide morphology, regulating the matrix strength and plasticity, and finally promoting further softening of the wire rod structure through roller slow cooling. Compared with the offline salt bath process, it can avoid brittle fracture of coiling and simplify the process steps, realize wire rod structure regulation, high strength and high plasticity matching, and has good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0035] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;
[0036] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;
[0037] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION
[0038] The embodiments described below with reference to the accompanying drawings are exemplary and are only for the purpose of illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention, but should not be construed as limiting the scope of the present invention. Embodiment 1:
[0039] A preferred embodiment of the manufacturing method of the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.82%, Si: 0.15%, Mn: 0.63%, P: 0.013%, S: 0.012%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt phase change regulation → roller slow cooling → coiling, specifically:
[0040] The controlled rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, select a lower heating furnace temperature and a shorter furnace time to control the decarburization degree of the high-carbon steel billet, and then roll the steel billet from the heating furnace into a wire with a diameter of 8mm through a rolling line, use a higher rolling temperature to reduce the wear of the rolling line and increase the rolling speed, and select a larger reduction to create favorable conditions for refining the organization and controlling the network carbide. Specifically: Control heating The furnace temperature is 1070°C, the furnace time is 3h, the oxygen content in the furnace is ≤1.3%, the initial rolling temperature is 1045°C, the initial rolling reduction is 26%, the final rolling temperature is 970°C, and the final rolling reduction is 38%; the wire-spinning process is used to make the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the secondary carbon precipitation of the wire rods and form a larger degree of supercooling, thereby promoting the nucleation of bainite and troostite. Specifically, the wire-spinning temperature is controlled to be 945°C.
[0041] The online molten salt phase change control adopts two salt baths with molten salt inside. The wire rod after spinning is first conveyed by rollers through the first salt bath, i.e., the first section of molten salt, and quickly cooled to the molten salt temperature. A lower isothermal temperature is selected to cool the wire rod at a cooling rate of 44°C / s, and quickly pass through the secondary carbon precipitation interval to promote the transformation of part of the high-temperature austenite to bainite and troostite structure to ensure the strength and plasticity of the matrix. The wire rod passing through the first section of molten salt is then conveyed by rollers through the second salt bath. The tank is the final molten salt, which is heated to the isothermal pearlite phase region to promote the transformation of untransformed high-temperature austenite to pearlite, and at the same time promote the tempering and softening of bainite, troostite and pearlite. Specifically: the molten salt temperature of the first molten salt is 442°C, the processing time is 8s, the molten salt circulation volume is 400t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the final molten salt is 500°C, the processing time is 350s, the molten salt circulation volume is 480t / h, and the molten salt temperature rise is ≤5°C.
[0042] The roller slow cooling process adopts closing the insulation cover to form an insulation channel structure, and uses the insulation roller to transport the wire rod coming out of the second salt bath tank into the insulation cover, and performs slow cooling treatment on the wire rod to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 286°C at a cooling rate of 0.65°C / s, and then coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and after packaging and storage, a cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 1 shown.
[0043] Comparative Example 1:
[0044] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of controlled rolling → low-temperature wire spinning → Stelmor insulation and slow cooling, specifically: the heating furnace temperature is controlled to 990°C, the furnace time is 5h, the initial rolling temperature is 950°C, the final rolling temperature is 840°C, the wire spinning temperature is 820°C, the Stelmor insulation and slow cooling adopts closing all fans and insulation covers, and the wire rod is conveyed by rollers. The wire rod completes phase change in the cover at a cooling rate of 1.2°C / s, and the finished wire rod is obtained after it comes off the line.
[0045] Comparative Example 2:
[0046] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to a process flow of controlled rolling → low-temperature wire spinning → air cooling → Stelmor insulation slow cooling, specifically: controlling the heating furnace temperature to 1000°C, the furnace time to 4h, the initial rolling temperature to 990°C, the final rolling temperature to 885°C, the wire spinning temperature to 860°C, the air cooling adopts opening a heat preservation cover, closing a fan, and conveying the wire rod with a roller, so that the wire rod is cooled to 685°C at a cooling rate of 2.2°C / s, the Stelmor insulation slow cooling adopts closing a fan and a heat preservation cover, conveying the wire rod with a roller, and the wire rod completes a phase change in the cover at a cooling rate of 0.9°C / s, and a finished wire rod is obtained after going offline.
[0047] Comparative Example 3:
[0048] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of controlled rolling → spinning → Stelmor rapid cooling + insulation slow cooling, specifically: controlling the heating furnace temperature to 1035°C, the furnace time to 4h, the initial rolling temperature to 1015°C, the final rolling temperature to 935°C, the spinning temperature to 910°C, the Stelmor rapid cooling + insulation slow cooling uses 1~7# fans to open at 45%, so that the wire rod is cooled to 690°C at a cooling rate of 5.8°C / s, then the rear fan and insulation cover are closed, the wire rod is conveyed by a roller, the wire rod completes phase change in the cover at a cooling rate of 0.6°C / s, and the finished wire rod is obtained after it comes off the line.
[0049] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organization and performance testing: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:
[0050] Table 1. Comparison of wire rod structure and properties by different manufacturing methods
[0051]
[0052] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with the high carbon carbon component design using high C-Si-Mn, under the low-temperature spinning and heat preservation slow cooling process, the obtained troostite + ferrite structure has higher wire rod strength, but the network carbide deterioration phase is formed in the process, which will destroy the continuity of the organization. The interlamellar spacing of the obtained troostite structure is large, and the organization stress and dislocation density are high, which makes the wire rod ultimately insufficient in plasticity, poor in cold deformation ability, and easy to draw harden. The present invention combines the high carbon carbon component design with the online molten salt phase change control technology to suppress the formation of network carbides at an ultra-fast cooling rate, effectively improve the economic value of the carbon element, and promote the transformation of part of the high-temperature austenite to bainite and troostite structure to ensure the strength and plasticity of the matrix, and then tempers and softens it through the final molten salt to continuously reduce the matrix dislocation density and adjust the carbide morphology, thereby achieving high strength and high plasticity matching.
[0053] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with slightly increasing the spinning temperature and then adopting air cooling and insulation cooling, the improvement on the net carbon is limited. At the same time, bainite, as a hard and brittle phase structure with high distortion and dislocation density, is difficult to soften during the continuous cooling process of insulation treatment on the Stelmor air cooling line, which easily leads to material waste and a decrease in the yield rate. The tempered bainite of the present invention retains the characteristic that bainite has higher strength than soft phase structures such as pearlite and ferrite. After being transformed into tempered bainite through tempering, the dislocation density is further reduced, so that the plasticity is significantly improved.
[0054] From the comparison results of Example 1 and Comparative Example 3, it can be seen that compared with further increasing the spinning temperature and then adopting air cooling for rapid cooling and heat preservation cooling, the improvement on the mesh carbon is limited, which will increase the risk of precipitation of abnormal tissues such as martensite and bainite that deteriorate the drawing performance, resulting in brittle fracture and difficulty in coiling of the finished product. The present invention can avoid the occurrence of abnormal martensitic tissue in the wire rod, reduce the fluctuation of the mechanical properties of the wire rod, and compensate for the adverse effects of high carbon content and bainite hard and brittle phase tissue on cold deformation performance. Embodiment 2:
[0055] A preferred embodiment of the manufacturing method of the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.83%, Si: 0.23%, Mn: 0.67%, P: 0.013%, S: 0.014%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt phase change regulation → roller slow cooling → coiling, specifically:
[0056] The controlled rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, select a lower heating furnace temperature and a shorter furnace time, control the decarburization degree of the high-carbon steel billet, and then roll the steel billet out of the heating furnace into a wire with a diameter of 10mm through a rolling line, use a higher rolling temperature to reduce the wear of the rolling line and increase the rolling speed, and select a larger reduction to create favorable conditions for refining the organization and controlling the network carbide. Specifically: control the heating furnace The temperature is 1085°C, the time in the furnace is 3.5h, the oxygen content in the furnace is ≤1.2%, the initial rolling temperature is 1065°C, the initial rolling reduction is 22%, the final rolling temperature is 980°C, and the final rolling reduction is 36%; the wire-spinning process is used to make the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the secondary carbon precipitation of the wire rods and form a larger degree of supercooling, thereby promoting the nucleation of bainite and troostite. Specifically, the wire-spinning temperature is controlled to be 950°C.
[0057] The online molten salt phase change control adopts two salt baths with molten salt inside. The wire rod after spinning is first conveyed by rollers through the first salt bath, i.e., the first section of molten salt, and quickly cooled to the molten salt temperature. A lower isothermal temperature is selected to cool the wire rod at a cooling rate of 44°C / s, and quickly pass through the secondary carbon precipitation interval to promote the transformation of part of the high-temperature austenite to bainite and troostite structure to ensure the strength and plasticity of the matrix. The wire rod passing through the first section of molten salt is then conveyed by rollers through the second salt bath. The tank is the final molten salt, which is heated to the isothermal state of the pearlite phase region to promote the transformation of untransformed high-temperature austenite to pearlite, and at the same time promote the tempering and softening of bainite, troostite and pearlite. Specifically: the molten salt temperature of the first molten salt is 450°C, the processing time is 5s, the molten salt circulation volume is 350t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the final molten salt is 472°C, the processing time is 400s, the molten salt circulation volume is 350t / h, and the molten salt temperature rise is ≤5°C.
[0058] The roller slow cooling process adopts closing the insulation cover to form an insulation channel structure, and uses the insulation roller to transport the wire rod coming out of the second salt bath tank into the insulation cover, and performs a slow cooling treatment on the wire rod to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 284°C at a cooling rate of 0.5°C / s, and then coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and after packaging and storage, a cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 2 shown.
[0059] Comparative Example 4:
[0060] A method for manufacturing a wire rod, which differs from that of Example 2 in that the heating furnace temperature is controlled to be 1040°C, the furnace time is 4 hours, the initial rolling temperature is 1020°C, the final rolling temperature is 940°C, the spinning temperature is 920°C, and the wire rod after spinning is first conveyed by a roller through a first section of molten salt, so that the wire rod is cooled at a cooling rate of 39°C / s, and the finished wire rod is obtained after it comes off the line.
[0061] Comparative Example 5:
[0062] A method for manufacturing wire rod, which differs from Example 2 in that the online molten salt phase change control adopts a salt bath tank with molten salt inside, and the wire rod after spinning is conveyed by a roller through the salt bath tank, so that the wire rod is cooled at a cooling rate of 42°C / s, the molten salt temperature is 465°C, the processing time is 405s, and the finished wire rod is obtained after going offline.
[0063] Comparative Example 6:
[0064] A method for manufacturing wire rods, which differs from that of Example 2 in that the wire rods after spinning are first conveyed by rollers through a first section of molten salt, so that the wire rods are cooled at a cooling rate of 48°C / s, the molten salt temperature of the first section of molten salt is 410°C, the processing time is 20s, the molten salt circulation rate is 500t / h, and the finished wire rods are obtained after going offline. Embodiment 3:
[0065] A preferred embodiment of the manufacturing method of the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.81%, Si: 0.2%, Mn: 0.58%, P: 0.015%, S: 0.014%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt phase change regulation → roller slow cooling → coiling, specifically:
[0066] The controlled rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, select a lower heating furnace temperature and a shorter furnace time, control the decarburization degree of the high-carbon steel billet, and then roll the steel billet out of the heating furnace into a wire with a diameter of 5.5mm through a rolling line, use a higher rolling temperature to reduce the wear of the rolling line and increase the rolling speed, and select a larger reduction to create favorable conditions for refining the organization and controlling the network carbide. Specifically: controlling the heating The hot furnace temperature is 1050°C, the furnace time is 2h, the oxygen content in the furnace is ≤1.4%, the initial rolling temperature is 1030°C, the initial rolling reduction is 28%, the final rolling temperature is 950°C, and the final rolling reduction is 42%; the wire-spinning process is used to make the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the secondary carbon precipitation of the wire rods and form a larger degree of supercooling, thereby promoting the nucleation of bainite and troostite. Specifically, the wire-spinning temperature is controlled to be 935°C.
[0067] The online molten salt phase change control adopts two salt baths with molten salt inside. The wire rod after spinning is first conveyed by rollers through the first salt bath, i.e., the first section of molten salt, and quickly cooled to the molten salt temperature. A lower isothermal temperature is selected to cool the wire rod at a cooling rate of 45°C / s, and quickly pass through the secondary carbon precipitation interval to promote the transformation of part of the high-temperature austenite to bainite and troostite structure to ensure the strength and plasticity of the matrix. The wire rod passing through the first section of molten salt is then conveyed by rollers through the second salt bath. The tank is the final molten salt, which is heated to the isothermal pearlite phase region to promote the transformation of untransformed high-temperature austenite to pearlite, and at the same time promote the tempering and softening of bainite, troostite and pearlite. Specifically: the molten salt temperature of the first molten salt is 420°C, the processing time is 15s, the molten salt circulation volume is 550t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the final molten salt is 520°C, the processing time is 270s, the molten salt circulation volume is 550t / h, and the molten salt temperature rise is ≤5°C.
[0068] The roller slow cooling process adopts closing the insulation cover to form an insulation channel structure, and uses the insulation roller to transport the wire rod coming out of the second salt bath tank into the insulation cover, and performs slow cooling treatment on the wire rod to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 295°C at a cooling rate of 0.8°C / s, and then coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and after packaging and storage, a cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 3 shown.
[0069] Comparative Example 7:
[0070] A method for manufacturing a wire rod, the manufacturing method of which is different from that of Example 3 in that the molten salt temperature of the final molten salt is 455° C., and a finished wire rod is obtained after the wire rod is off the production line.
[0071] Comparative Example 8:
[0072] A method for manufacturing a wire rod, which differs from Example 3 in that the molten salt temperature of the final molten salt is 535°C, the processing time is 420s, the molten salt circulation rate is 600t / h, and a finished wire rod is obtained after going offline.
[0073] Comparative Example 9:
[0074] A method for manufacturing a wire rod, which differs from Example 3 in that the processing time of the final molten salt is 165s, and a finished wire rod is obtained after the wire rod is offline. Embodiment 4:
[0075] A preferred embodiment of the manufacturing method of the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.79%, Si: 0.25%, Mn: 0.72%, P: 0.014%, S: 0.015%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt phase change regulation → roller slow cooling → coiling, specifically:
[0076] The controlled rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, select a lower heating furnace temperature and a shorter furnace time to control the decarburization degree of the high-carbon steel billet, and then roll the steel billet out of the heating furnace into a wire with a diameter of 12mm through a rolling line, use a higher rolling temperature to reduce the wear of the rolling line and increase the rolling speed, and select a larger reduction to create favorable conditions for refining the organization and controlling the network carbide. Specifically: Control heating The furnace temperature is 1100°C, the furnace time is 4h, the oxygen content in the furnace is ≤1.4%, the initial rolling temperature is 1075°C, the initial rolling reduction is 20%, the final rolling temperature is 990°C, and the final rolling reduction is 32%; the wire-spinning process is used to make the wire rods coming out of the rolling line into wire rods through a wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the secondary carbon precipitation of the wire rods and form a larger degree of supercooling, thereby promoting the nucleation of bainite and troostite. Specifically, the wire-spinning temperature is controlled to be 965°C.
[0077] The online molten salt phase change control adopts two salt baths with molten salt inside. The wire rod after spinning is first conveyed by rollers through the first salt bath, i.e., the first section of molten salt, and quickly cooled to the molten salt temperature. A lower isothermal temperature is selected to cool the wire rod at a cooling rate of 47°C / s, and quickly pass through the secondary carbon precipitation interval to promote the transformation of part of the high-temperature austenite to bainite and troostite structure to ensure the strength and plasticity of the matrix. The wire rod passing through the first section of molten salt is then conveyed by rollers through the second salt bath. The tank is the final molten salt, which is heated to the isothermal state of the pearlite phase region to promote the transformation of untransformed high-temperature austenite to pearlite, and at the same time promote the tempering and softening of bainite, troostite and pearlite. Specifically: the molten salt temperature of the first molten salt is 430°C, the processing time is 12s, the molten salt circulation volume is 500t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the final molten salt is 460°C, the processing time is 200s, the molten salt circulation volume is 380t / h, and the molten salt temperature rise is ≤5°C.
[0078] The roller slow cooling process adopts closing the insulation cover to form an insulation channel structure, and uses the insulation roller to transport the wire rod coming out of the second salt bath tank into the insulation cover, and inputs the hot air generated during the online molten salt phase change regulation process into the insulation cover to perform slow cooling on the wire rod to promote further softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled to 295°C at a cooling rate of 0.35°C / s, and then coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage.
[0079] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 10 were subjected to organization and performance testing: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:
[0080] Table 2. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods
[0081]
[0082] It can be seen from the results of Examples 1 to 4 that the cold heading steel wire rod of the present invention adopts a high carbon carbon component design with high C-Si-Mn, which can save alloy components such as Cr, Mo, Ti, V, Nb, B, and Ni, effectively reducing material costs. The microstructure includes most tempered pearlite, a small part of tempered troostite, a small amount of tempered bainite and fused pearlite, but does not include martensite structure, achieving high strength and high plasticity matching, reaching a tensile strength of 1305~1345MPa, and a cross-sectional reduction rate of 44%~49%. It can be suitable for efficient and green manufacturing of 14.9 grade bolts under non-quenching and tempering process, reducing carbon emissions and bolt costs.
[0083] From the comparison results of Example 2 and Comparative Example 4, it can be seen that by selecting a higher spinning temperature and utilizing the high heat exchange capacity of the molten salt to cool the wire rod extremely quickly, the inhibition of the network carbide can be effectively avoided, and favorable conditions are provided for promoting the troostite phase transformation with finer interlamellar spacing. From the comparison results of Example 2 and Comparative Example 5, it can be seen that the use of a salt bath treatment is equivalent to increasing the molten salt temperature of the first stage molten salt. The higher the molten salt temperature and the shorter the time, the smaller the proportion of tempered bainite, the larger the interlamellar spacing of the troostite, The strength of the wire rod decreases and the plasticity increases, but the molten salt temperature is too high and the time is too short, which is not conducive to the bainite transformation and the matrix strength is significantly lost; from the comparison results of Example 2 and Comparative Example 6, it can be seen that the lower the molten salt temperature of the first stage of the molten salt and the longer the treatment time, the more austenite transforms to bainite, the finer the spacing between the troostite lamellae, the higher the proportion of tempered bainite, the strength of the wire rod increases and the plasticity decreases, but the molten salt temperature of the first stage of the molten salt is too low and the time is too long, the proportion of tempered bainite is too high, which is not conducive to the plasticity of the wire rod.
[0084] From the comparison results of Example 3 and Comparative Example 7, it can be seen that the lower the molten salt temperature of the final molten salt, the finer the spacing between the pearlite lamellae formed, but if the molten salt temperature is too low, the proportion of troostite will increase due to supercooling, which will affect the plasticity of the wire rod; from the comparison results of Example 3 and Comparative Example 8, it can be seen that the higher the molten salt temperature, the coarser the spacing between the pearlite lamellae formed, which can provide more thermal power for the tempering and softening of bainite, troostite and pearlite structures, so that the strength of the wire rod decreases and the plasticity increases, but too high a molten salt temperature can easily cause the lamellae to be too coarse and excessive tempering and softening, which is not good for the strength of the wire rod; from the comparison results of Example 3 and Comparative Example 9, it can be seen that the shorter the processing time, the worse the tempering and softening effect, and the plasticity of the wire rod decreases; from the comparison results of Example 4 and Comparative Example 10, it can be seen that after slow cooling on a roller, the high temperature state of the wire rod after passing through the molten salt can be used to promote the one-step softening of the tempered bainite, troostite and pearlite structures.
[0085] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.79% to 0.83%, Si: 0.15% to 0.25%, Mn: 0.58% to 0.72%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities; its microstructure includes 50% to 60% by volume of tempered pearlite, 5% to 10% by volume of tempered bainite, 25% to 35% by volume of tempered troostite, and the rest is a mixed structure composed of fused pearlite, and its manufacturing method includes: The wire rod is produced by controlled rolling according to the chemical composition of the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod. After the wire rod is spun into a wire rod at a spinning temperature of ≥935°C, an online molten salt phase transformation control is performed, so that the wire rod first passes through the first section of molten salt, and the wire rod is cooled at a cooling rate of ≥44°C / s to the bainite and troostite phase region for organizational phase transformation, promoting the transformation of part of austenite to bainite and troostite, and then the wire rod passes through the final section of molten salt and is heated to the pearlite phase region isotherm, promoting the transformation of untransformed austenite to pearlite, while promoting the transformation of bainite, troostite and The pearlite is tempered and softened, and finally slowly cooled by a roller to obtain a cold heading steel wire rod having a mixed structure consisting of tempered pearlite, tempered bainite, tempered troostite and fused pearlite. The molten salt temperature of the first molten salt is 420-450°C, and the processing time is 5-15s. The molten salt temperature of the last molten salt is 460-520°C, and the processing time is 200-400s. The roller slow cooling adopts a closed heat preservation cover to control the wire rod to be cooled to below 300°C at a cooling rate of 0.35-0.80°C / s.
2. The 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 155-185 nm, the interlamellar spacing of the tempered troostite is 75-105 nm, and the network carbide level of the cold heading steel wire rod is level 0.
3. The 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts according to claim 1, characterized in that: The cold heading steel wire rod has a diameter of 5.5-12.0 mm, a tensile strength of 1305-1345 MPa, and a cross-sectional shrinkage of 44%-49%.
4. A method for manufacturing a high carbon cold heading steel wire rod for 14.9 grade non-quenched and tempered bolts, characterized in that: The manufacturing method comprises: producing a wire rod by controlled rolling according to the chemical composition of the 14.9-grade non-quenched and tempered high-carbon cold heading steel wire rod for bolts as claimed in claim 1, after the wire rod is spun into a wire rod at a spinning temperature of ≥935°C, performing online molten salt phase transformation control, so that the wire rod first passes through a first section of molten salt, the wire rod is cooled at a cooling rate of ≥44°C / s to a bainite and troostite phase region for structural phase transformation, promoting the transformation of part of austenite into bainite and troostite, the wire rod is then heated to an isothermal pearlite phase region through a final section of molten salt, promoting the transformation of untransformed austenite into pearlite, and promoting the tempering and softening of bainite, troostite and pearlite, and finally passing through a roller for slow cooling , a cold heading steel wire rod having a mixed structure of 50% to 60% by volume of tempered pearlite, 5% to 10% by volume of tempered bainite, 25% to 35% by volume of tempered troostite, and the rest being fused pearlite; the molten salt temperature of the first section of molten salt is 420 to 450°C, and the processing time is 5 to 15s; the molten salt temperature of the last section of molten salt is 460 to 520°C, and the processing time is 200 to 400s; the roller slow cooling adopts closing the heat preservation cover, and controls the wire rod to be cooled to below 300°C at a cooling rate of 0.35 to 0.80°C / s.
5. The method for manufacturing the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts according to claim 4, characterized in that: During the controlled rolling, the temperature of the heating furnace is controlled to be 1050-1100° C. before rolling, the time in the furnace is 2-4 hours, and the oxygen content in the furnace is ≤1.4%.
6. The method for manufacturing the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts according to claim 4, characterized in that: During the controlled rolling, the initial rolling temperature is controlled to be 1030-1075° C., the initial rolling reduction is 20%-28%, the final rolling temperature is ≥950° C., and the final rolling reduction is 32%-42%.
7. The method for manufacturing the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts according to claim 4, characterized in that: The molten salt circulation rate of the first stage molten salt is 350-550t / h, and the temperature rise of the molten salt is ≤10°C.
8. The method for manufacturing the 14.9 grade non-quenched and tempered high carbon cold heading steel wire rod for bolts according to claim 4, characterized in that: The molten salt circulation rate of the final stage molten salt is 350-550t / h, and the molten salt temperature rise is ≤5°C.
Citation Information
Cited By
Delayed-fracture-resistant non-quenched-tempered 14.9-grade high-strength cold heading steel wire rod and preparation method thereof
CN121228119A