Environmentally friendly ohmic silver paste for PTC heater of new energy vehicles and preparation method thereof

Through the combination of high-purity nano silver powder, nano zinc powder and high-temperature binder matching thermal expansion coefficient, the problem of traditional ohmic silver paste with low pressure resistance and non-impact resistance in PTC heaters of new energy vehicles is solved, and efficient thermal management is achieved Performance and environmentally friendly conductive silver paste preparation.

CN118645284BActive Publication Date: 2024-12-06WUHAN YILAI RUIER HIGH TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410984891.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-12-06
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Traditional ohmic silver paste is low pressure resistant, not impact resistant, has a large heat attenuation in PTC heaters of new energy vehicles, and is highly polluted to the environment, which cannot meet the durability requirements of high pressure and long-term thermal aging.

Method used

The high-purity nano silver powder and high-purity nano zinc powder combined with high-temperature binder close to the thermal expansion coefficient is prepared by tank grinding and ultrasonic dispersion, and the silica content is optimized through genetic algorithm to match the thermal expansion of ceramics. coefficient, forming good adhesion and conductivity.

Benefits of technology

It significantly improves the voltage, impact and thermal management performance of conductive silver paste, meets the requirements of the PTC thermal management system of new energy vehicles, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_67
    Figure SMS_67
Patent Text Reader

Abstract

The present invention belongs to the technical field of conductive silver paste preparation, and specifically relates to an environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof. The technical key points are as follows: calculated by weight, it includes the following components: 40 to 58 parts of high-purity nano silver powder, 10 to 20 parts of high-purity nano zinc powder, 5 to 30 parts of a high-temperature binder, 5 to 20 parts of an active additive, 5 to 15 parts of an antioxidant stabilizer, 3 to 5 parts of a dispersing defoaming agent, and 10 to 28 parts of an organic carrier; wherein the thermal expansion coefficient of the high-temperature binder matches the thermal expansion coefficient of ceramics used in the PTC heater. The environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle provided by the present invention and a preparation method thereof introduce a large amount of nanomaterials, and introduce a high-temperature heat-resistant glass powder binder component that is extremely close to the thermal expansion coefficient of automotive PTC ceramics, thereby overcoming the fatal defects of traditional ohmic silver paste, such as low pressure resistance, poor impact resistance, large thermal attenuation, and poor reliability, and fully meeting the various performance requirements of the PTC thermal management system for new energy vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive silver paste preparation, and specifically relates to an environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof. Background Art

[0002] Silver electrode paste is made of ultrafine silver powder, glass binder, organic carrier and additives. Ultrafine silver powder is responsible for conducting electricity in the electrode; the glass binder melts during the sintering process and fixes the metal conductive powder on the surface of the substrate, thus forming a uniform conductive film with a thickness of 10μm to 12μm; the organic carrier is used to disperse the paste to ensure that it has good fluidity and thixotropy, making the paste a stable suspension that can be placed for a long time without precipitation; the additives are used to improve the adhesion, surface morphology and structure of the conductive film after sintering.

[0003] At present, the glass binder used in the commonly used low-temperature sintering silver electrode paste is a boron-silicon-lead glass, which has a low melting point, good melting fluidity and excellent substrate material wettability. However, the lead content in this material is relatively high, usually exceeding 50% in the glass composition, causing significant pollution to the environment.

[0004] The commonly used lead-free conductive silver paste has only general ohmic contact characteristics and cannot meet the durability requirements of the PTC heater for new energy vehicles, such as high voltage resistance (800~1200V), impact resistance, and long-term thermal aging. Summary of the invention

[0005] The purpose of the present invention is to provide an environmentally friendly ohmic silver paste for PTC heaters of new energy vehicles and a preparation method thereof, which introduces a large amount of nanomaterials and a high-temperature heat-resistant glass powder binder component whose thermal expansion coefficient is extremely close to that of automotive PTC ceramics, thereby overcoming the fatal defects of traditional ohmic silver paste, such as low pressure resistance, poor impact resistance, large thermal attenuation and poor reliability, and fully meeting the various performance requirements of the PTC thermal management system for new energy vehicles.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions:

[0007] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided by the present invention is characterized in that it comprises the following components calculated by weight:

[0008] 40-58 parts of high-purity nano silver powder, 10-20 parts of high-purity nano zinc powder, 5-30 parts of high-temperature binder, 5-20 parts of active additive, 5-15 parts of antioxidant stabilizer, 3-5 parts of dispersing defoaming agent and 10-28 parts of organic carrier;

[0009] Wherein, the thermal expansion coefficient of the high temperature adhesive matches the thermal expansion coefficient of the ceramic used for the PTC heater.

[0010] Furthermore, the silver content of the high-purity nano silver powder after calcination is 99.95%, the particle size range is 50~200nm, and the sphericity is ≥80%.

[0011] Furthermore, the purity of the high-purity nano zinc powder is ≥99.9%, the particle size range is 100~300nm, and the sphericity is ≥85%.

[0012] Furthermore, the high temperature adhesive is any one of the rare earth oxide modified phosphate, bismuth, and vanadate heat-resistant or water-resistant glass systems.

[0013] Furthermore, the active additive is an inorganic nano-semi-metal element single substance with a particle size of 50~100nm.

[0014] Furthermore, the organic carrier includes a polymer resin and a solvent.

[0015] Furthermore, the polymer resin is ethyl cellulose or nitrocellulose; and the solvent is any one of butyl ether, cyclohexanone or turpentine.

[0016] Furthermore, the mass ratio of the polymer resin to the solvent is 1:(3~5).

[0017] Furthermore, the antioxidant stabilizer is any one of phthalate, aluminate or zincate.

[0018] Furthermore, the dispersing defoaming agent is any one of lecithin, synthetic phosphate ester or silicone defoaming agent.

[0019] Furthermore, the content of silicon dioxide in the high-temperature adhesive is determined according to the thermal expansion coefficient of the ceramic used in the PTC heater.

[0020] Furthermore, the content of silicon dioxide in the high-temperature adhesive is determined according to the thermal expansion coefficient of the ceramic for the PTC heater, specifically including: setting a threshold value for the difference between the thermal expansion coefficient of the high-temperature adhesive and the thermal expansion coefficient of the ceramic for the PTC heater; determining the thermal expansion coefficient of the high-temperature adhesive according to the threshold value and the thermal expansion coefficient of the ceramic for the PTC heater; and then determining the content of silicon dioxide in the high-temperature adhesive using a genetic algorithm according to the thermal expansion coefficient of the high-temperature adhesive.

[0021] The present invention also provides a method for preparing an environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle, comprising the following steps:

[0022] Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight proportions and put them into a pot mill, pot mill for 40h to 48h, and then obtain a premixed powder after ultrasonic dispersion and sieving;

[0023] Active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers are added to the premixed powder, and the premixed powder is ground through a three-roll mill.

[0024] In summary, the present invention has the following beneficial effects:

[0025] The environmentally friendly ohmic silver paste for PTC heaters of new energy vehicles and the preparation method thereof provided by the present invention introduce a large amount of nanomaterials and a high-temperature heat-resistant glass powder binder component whose thermal expansion coefficient is extremely close to that of automotive PTC ceramics, thereby overcoming the fatal defects of traditional ohmic silver paste such as low pressure resistance, poor impact resistance, large thermal attenuation and poor reliability, and fully meeting the various performance requirements of the PTC thermal management system for new energy vehicles. DETAILED DESCRIPTION

[0026] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the environmentally friendly ohmic silver paste for the PTC heater of new energy vehicles proposed in the present invention and its preparation method, its specific implementation method, characteristics and effects are described in detail as follows.

[0027] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided in this specific embodiment includes the following components calculated by weight:

[0028] 40-58 parts of high-purity nano silver powder, 10-20 parts of high-purity nano zinc powder, 5-30 parts of high-temperature binder, 5-20 parts of active additive, 5-15 parts of antioxidant stabilizer, 3-5 parts of dispersing defoaming agent and 10-28 parts of organic carrier;

[0029] Among them, the thermal expansion coefficient of the high temperature adhesive matches the thermal expansion coefficient of the ceramic used in the PTC heater.

[0030] In this specific embodiment, when the thermal expansion coefficients of the PTC ceramic and the binder are similar, their expansion and contraction degrees when the temperature changes will also be similar. This matching helps to reduce the thermal stress caused by temperature changes, thereby avoiding cracking or peeling of the material.

[0031] At the same time, similar thermal expansion coefficients can ensure good contact and strong bonding between the adhesive and the ceramic. Under temperature changes, the adhesive and the ceramic can expand and contract evenly, maintaining a stable contact surface and avoiding shedding or failure of the bonding interface.

[0032] For example, the silver content of high-purity nano silver powder after calcination is 99.95%, the particle size range is 50~200nm, and the sphericity is ≥80%; the silver powder that meets the above conditions has good low-temperature activity, can interpenetrate and melt with ohmic metal to form alloy components when co-fired, and has excellent conductivity, extremely high voltage resistance, and great resistance to current shock.

[0033] For example, the purity of high-purity nano zinc powder is ≥99.9%, the particle size range is 100~300nm, and the sphericity is ≥85%; the zinc powder that meets the above conditions has extremely strong ohmic contact activity, can quickly interpenetrate and melt with nano silver powder to form an alloy, and form good ohmic contact with the PTC ceramic body.

[0034] For example, the high temperature binder is any one of the rare earth oxide modified phosphate, bismuth, vanadate heat-resistant or water-resistant glass systems. These glasses are melted at a high temperature of 1200°C, then water quenched and ball-milled to form a glass powder high temperature binder with a fineness of 1-3 μm. The high temperature binder can form a good sintering infiltration with the PTC ceramic body, penetrate into the ceramic grain boundary, melt into one, and form a very strong chemical bonding force and mechanical bonding force.

[0035] For example, the active additive is an inorganic nano-semi-metallic element with a nanoparticle size of 50~100nm; specifically, it can be a single element such as boron and silicon. These added single elements can form an alloy with the silver and zinc components, and have good stability and thermal creep resistance, so that the ohmic electrode has good anti-aging durability.

[0036] Illustratively, the organic vehicle includes a polymer resin and a solvent.

[0037] Specifically, the polymer resin is ethyl cellulose or nitrocellulose; and the solvent is any one of butyl ether, cyclohexanone or turpentine.

[0038] More specifically, the mass ratio of polymer resin to solvent is 1:(3~5).

[0039] Illustratively, the antioxidant stabilizer is any one of phthalate, aluminate or zincate.

[0040] Illustratively, the dispersing defoaming agent is any one of lecithin, synthetic phosphate ester or silicone-based defoaming agent.

[0041] For example, the content of silicon dioxide in the high-temperature binder is determined according to the thermal expansion coefficient of the ceramic used in the PTC heater; by adjusting the content of silicon dioxide in the high-temperature binder, its thermal expansion coefficient can be effectively improved to make it closer to the thermal expansion coefficient of the PTC ceramic. This adjustment can help reduce the stress caused by thermal expansion mismatch and improve the overall performance and durability of the heater.

[0042] In this specific embodiment, the content of silicon dioxide in the high-temperature adhesive is determined based on the thermal expansion coefficient of the ceramic for the PTC heater, specifically including: setting a threshold value for the difference between the thermal expansion coefficient of the high-temperature adhesive and the thermal expansion coefficient of the ceramic for the PTC heater; determining the thermal expansion coefficient of the high-temperature adhesive based on the threshold value and the thermal expansion coefficient of the ceramic for the PTC heater; and then determining the content of silicon dioxide in the high-temperature adhesive using a genetic algorithm based on the thermal expansion coefficient of the high-temperature adhesive.

[0043] Specifically, the content of silicon dioxide in the high-temperature adhesive is determined by using a genetic algorithm according to the thermal expansion coefficient of the high-temperature adhesive, including the following steps:

[0044] Collect the component formulas of different types of high-temperature adhesives;

[0045] Collect the thermal expansion coefficient of high temperature adhesives at different silica contents;

[0046] Based on the thermal expansion coefficient data of high-temperature adhesives, a thermal expansion coefficient scoring model is established, and corresponding constraints are constructed;

[0047] Based on the thermal expansion coefficient scoring model and corresponding constraint conditions, the genetic algorithm is used to optimize the silica content of the high-temperature adhesive and obtain the optimal silica content of the high-temperature adhesive.

[0048] More specifically, the constraint condition is that the threshold of the difference between the thermal expansion coefficient of the high temperature adhesive and the thermal expansion coefficient of the PTC heater ceramic is within a set value range. According to the actual situation, the set value range is .

[0049] The method for preparing an environmentally friendly ohmic silver paste for a PTC heater for a new energy vehicle provided in this specific embodiment comprises the following steps:

[0050] Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight proportions and put them into a pot mill, pot mill for 40h to 48h, and then obtain a premixed powder after ultrasonic dispersion and sieving;

[0051] Active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers are added to the premixed powder, and the premixed powder is ground through a three-roll mill.

[0052] Example 1: An environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof

[0053] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided in this embodiment includes the following components calculated by weight:

[0054] 45 parts of high-purity nano silver powder, 15 parts of high-purity nano zinc powder, 15 parts of high-temperature binder, 5 parts of active additives, 5 parts of antioxidants, 4 parts of dispersing defoaming agents and 11 parts of organic carriers.

[0055] The method for preparing the environmentally friendly ohmic silver paste for the PTC heater of the new energy vehicle provided in this embodiment comprises the following steps:

[0056] S1. Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight parts, put them into a pot mill, pot mill for 40 hours, and then disperse them through a 300-mesh sieve by ultrasonic to obtain a premixed powder;

[0057] S2. Add active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers to the premixed powder, and grind the premixed powder through a three-roll mill.

[0058] Among them, the silver content of high-purity nano silver powder after calcination is 99.95%, the particle size range is 50~200nm, and the sphericity is 87%; the purity of high-purity nano zinc powder is 99.9%, the particle size range is 100~300nm, and the sphericity is 89%; the active additive is boron element with a nanoparticle size of 50~100nm; the antioxidant stabilizer is aluminate; the dispersing and defoaming agent is lecithin dispersing and defoaming agent; the organic carrier is ethyl cellulose and butyl ether, with a mass ratio of 1:3.

[0059] The high-temperature binder is a phosphate glass modified by rare earth oxides, which is melted at 1200°C, then quenched with water and ball-milled into a glass powder with a fineness of 1-3 μm. Its components are as follows according to mass percentage: silicon dioxide 45.78%, aluminum phosphate 14.92%, monocalcium phosphate 9.67%, lanthanum oxide 5.14%, cerium oxide 5.14%, Tantalum oxide 5.14%, Germanium oxide 9.67% and sodium oxide 5.54%; thermal expansion coefficient is .

[0060] Among them, silicon dioxide The content is determined based on the thermal expansion coefficient using a genetic algorithm.

[0061] Example 2: An environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof

[0062] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided in this embodiment includes the following components calculated by weight:

[0063] 50 parts of high-purity nano silver powder, 10 parts of high-purity nano zinc powder, 13 parts of high-temperature adhesive, 6 parts of active additive, 6 parts of antioxidant, 3 parts of dispersing defoaming agent and 12 parts of organic carrier.

[0064] The method for preparing the environmentally friendly ohmic silver paste for the PTC heater of the new energy vehicle provided in this embodiment comprises the following steps:

[0065] S1. Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight parts, put them into a pot mill, pot mill for 40 hours, and then disperse them through a 300-mesh sieve by ultrasonic to obtain a premixed powder;

[0066] S2. Add active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers to the premixed powder, and grind the premixed powder through a three-roll mill.

[0067] Among them, the silver content of high-purity nano silver powder after calcination is 99.95%, the particle size range is 50~200nm, and the sphericity is 87%; the purity of high-purity nano zinc powder is 99.9%, the particle size range is 100~300nm, and the sphericity is 89%; the active additive is boron element with a nano particle size of 50~100nm; the antioxidant stabilizer is aluminate; the dispersing and defoaming agent is lecithin dispersing and defoaming agent.

[0068] The high-temperature binder is bismuthate glass, which is melted at 1200℃, then quenched and ball-milled into glass powder with a fineness of 1~3μm. Its components are as follows according to mass percentage: bismuthate 48.50%, silicon dioxide 25.25%, Alumina 8.10%, barium oxide 6.75%, Germanium oxide 4.50%, sodium oxide 3.90%, lead oxide 2.00% and magnesium oxide 1.00%; thermal expansion coefficient is .

[0069] Among them, silicon dioxide The content is determined based on the thermal expansion coefficient using a genetic algorithm.

[0070] Example 3: An environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof

[0071] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided in this embodiment includes the following components calculated by weight:

[0072] 42 parts of high-purity nano silver powder, 18 parts of high-purity nano zinc powder, 5 parts of high-temperature binder, 10 parts of active additive, 5 parts of antioxidant, 4 parts of dispersing defoaming agent, and 16 parts of organic carrier.

[0073] The method for preparing the environmentally friendly ohmic silver paste for the PTC heater of the new energy vehicle provided in this embodiment comprises the following steps:

[0074] S1. Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight parts, put them into a pot mill, pot mill for 40 hours, and then disperse them through a 300-mesh sieve by ultrasonic to obtain a premixed powder;

[0075] S2. Add active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers to the premixed powder, and grind the premixed powder through a three-roll mill.

[0076] Among them, the silver content of high-purity nano silver powder after calcination is 99.95%, the particle size range is 50~200nm, and the sphericity is 87%; the purity of high-purity nano zinc powder is 99.9%, the particle size range is 100~300nm, and the sphericity is 89%; the active additive is boron element with a nanoparticle size of 50~100nm; the antioxidant stabilizer is aluminate; the dispersing and defoaming agent is lecithin dispersing and defoaming agent; the organic carrier is ethyl cellulose and butyl ether, with a mass ratio of 1:3.

[0077] The high-temperature binder is a vanadate-based heat-resistant glass, which is melted at 1200°C, then quenched with water and ball-milled into a glass powder with a fineness of 1~3μm. Calculated by mass percentage, its components are as follows: Vanadate 43.67%, silicon dioxide 28.34%, Alumina 12.45%, barium oxide 6.78%, magnesium oxide 4.56%, Germanium oxide 2.89%, sodium oxide ( 1.85% and zinc oxide 1.46%.

[0078] Among them, silicon dioxide The content is determined based on the thermal expansion coefficient using a genetic algorithm.

[0079] Comparative Example 1: An environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof

[0080] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided in this embodiment includes the following components calculated by weight:

[0081] 45 parts of high-purity nano silver powder, 15 parts of high-purity nano zinc powder, 15 parts of high-temperature binder, 5 parts of active additives, 5 parts of antioxidants, 4 parts of dispersing defoaming agents and 11 parts of organic carriers.

[0082] The method for preparing the environmentally friendly ohmic silver paste for the PTC heater of the new energy vehicle provided in this embodiment comprises the following steps:

[0083] S1. Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight parts, put them into a pot mill, pot mill for 40 hours, and then disperse them through a 300-mesh sieve by ultrasonic to obtain a premixed powder;

[0084] S2. Add active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers to the premixed powder, and grind the premixed powder through a three-roll mill.

[0085] Among them, the silver content of high-purity nano silver powder after calcination is 99.95%, the particle size range is 50~200nm, and the sphericity is 87%; the purity of high-purity nano zinc powder is 99.9%, the particle size range is 100~300nm, and the sphericity is 89%; the active additive is boron element with a nanoparticle size of 50~100nm; the antioxidant stabilizer is aluminate; the dispersing and defoaming agent is lecithin dispersing and defoaming agent; the organic carrier is ethyl cellulose and butyl ether, with a mass ratio of 1:3.

[0086] The high-temperature binder is a phosphate glass modified by rare earth oxides, which is melted at 1200°C, then quenched with water and ball-milled into a glass powder with a fineness of 1-3 μm. Its components are as follows according to mass percentage: silicon dioxide 35.00%, aluminum phosphate 11.45%, monocalcium phosphate 7.63%, lanthanum oxide 4.11%, cerium oxide 4.11%, Tantalum oxide 4.11%, Germanium oxide 7.63% and sodium oxide 4.85%; Thermal expansion coefficient: .

[0087] Comparative Example 2: An environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof

[0088] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided in this embodiment includes the following components calculated by weight:

[0089] 50 parts of high-purity nano silver powder, 10 parts of high-purity nano zinc powder, 13 parts of high-temperature adhesive, 6 parts of active additive, 6 parts of antioxidant, 3 parts of dispersing defoaming agent and 12 parts of organic carrier.

[0090] The method for preparing the environmentally friendly ohmic silver paste for the PTC heater of the new energy vehicle provided in this embodiment comprises the following steps:

[0091] S1. Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight parts, put them into a pot mill, pot mill for 40 hours, and then disperse them through a 300-mesh sieve by ultrasonic to obtain a premixed powder;

[0092] S2. Add active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers to the premixed powder, and grind the premixed powder through a three-roll mill.

[0093] Among them, the silver content of high-purity nano silver powder after calcination is 99.95%, the particle size range is 50~200nm, and the sphericity is 87%; the purity of high-purity nano zinc powder is 99.9%, the particle size range is 100~300nm, and the sphericity is 89%; the active additive is boron element with a nanoparticle size of 50~100nm; the antioxidant stabilizer is aluminate; the dispersing and defoaming agent is lecithin dispersing and defoaming agent; the organic carrier is ethyl cellulose and butyl ether, with a mass ratio of 1:3.

[0094] The high-temperature binder is bismuth-based glass, which is melted at 1200°C, then quenched and ball-milled into glass powder with a fineness of 1-3 μm. Its components are as follows according to mass percentage: silicon dioxide 40.00%, bismuth acid 38.85%, Alumina 6.49%, barium oxide 5.41%, Germanium oxide 3.61%, sodium oxide 3.13%, lead oxide 1.60% and magnesium oxide 0.80%; thermal expansion coefficient is .

[0095] Comparative Example 3: An environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof

[0096] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided in this embodiment includes the following components calculated by weight:

[0097] 45 parts of high-purity nano silver powder, 15 parts of high-purity nano zinc powder, 15 parts of high-temperature binder, 5 parts of active additives, 5 parts of antioxidants, 4 parts of dispersing defoaming agents and 11 parts of organic carriers.

[0098] The method for preparing the environmentally friendly ohmic silver paste for the PTC heater of the new energy vehicle provided in this embodiment comprises the following steps:

[0099] S1. Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight parts, put them into a pot mill, pot mill for 40 hours, and then disperse them through a 300-mesh sieve by ultrasonic to obtain a premixed powder;

[0100] S2. Add active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers to the premixed powder, and grind the premixed powder through a three-roll mill.

[0101] Among them, the silver content of the nano silver powder after calcination is 85%, the particle size range is 50~200nm, and the sphericity is 76%; the purity of the high-purity nano zinc powder is 99.9%, the particle size range is 100~300nm, and the sphericity is 89%; the active additive is boron element with a nano particle size of 50~100nm; the antioxidant stabilizer is aluminate; the dispersing and defoaming agent is lecithin dispersing and defoaming agent; the organic carrier is ethyl cellulose and butyl ether, with a mass ratio of 1:3.

[0102] The high-temperature binder is a phosphate glass modified by rare earth oxides, which is melted at 1200°C, then quenched with water and ball-milled into a glass powder with a fineness of 1-3 μm. Its components are as follows according to mass percentage: silicon dioxide 45.78%, aluminum phosphate 14.92%, monocalcium phosphate 9.67%, lanthanum oxide 5.14%, cerium oxide 5.14%, Tantalum oxide 5.14%, Germanium oxide 9.67% and sodium oxide 5.54%; thermal expansion coefficient is .

[0103] Comparative Example 4: An environmentally friendly ohmic silver paste for a PTC heater of a new energy vehicle and a preparation method thereof

[0104] The environmentally friendly ohmic silver paste for the PTC heater of a new energy vehicle provided in this embodiment includes the following components calculated by weight:

[0105] 45 parts of high-purity nano silver powder, 15 parts of high-purity nano zinc powder, 15 parts of high-temperature binder, 5 parts of active additives, 5 parts of antioxidants, 4 parts of dispersing defoaming agents and 11 parts of organic carriers.

[0106] The method for preparing the environmentally friendly ohmic silver paste for the PTC heater of the new energy vehicle provided in this embodiment comprises the following steps:

[0107] S1. Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight parts, put them into a pot mill, pot mill for 40 hours, and then disperse them through a 300-mesh sieve by ultrasonic to obtain a premixed powder;

[0108] S2. Add active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers to the premixed powder, and grind the premixed powder through a three-roll mill.

[0109] Among them, the silver content of high-purity nano silver powder after calcination is 99.95%, the particle size range is 50~200nm, and the sphericity is 87%; the purity of nano zinc powder is 89.7%, the particle size range is 100~300nm, and the sphericity is 65%; the active additive is boron element with a nano particle size of 50~100nm; the antioxidant stabilizer is aluminate; the dispersing and defoaming agent is lecithin dispersing and defoaming agent.

[0110] The high-temperature binder is a phosphate glass modified by rare earth oxides, which is melted at 1200°C, then quenched with water and ball-milled into a glass powder with a fineness of 1-3 μm. Its components are as follows according to mass percentage: silicon dioxide 45.78%, aluminum phosphate 14.92%, monocalcium phosphate 9.67%, lanthanum oxide 5.14%, cerium oxide 5.14%, Tantalum oxide 5.14%, Germanium oxide 9.67% and sodium oxide 5.54%; thermal expansion coefficient is .

[0111] The conductive silver paste of Examples 1 to 3 and Comparative Examples 1 to 4 was printed on a PTC ceramic substrate through a stainless steel screen. After removing the screen, the samples were heated to 120° C. and dried for 40 min to obtain samples. The pressure resistance, high temperature adhesion and thermal attenuation properties of the samples were tested. The test method and test results are as follows.

[0112] High temperature adhesion: Heat the sample to 600℃ to test the adhesion between the conductive silver paste and the substrate.

[0113] Hi-pot test: Apply a gradually increasing DC voltage to the sample, starting from a low voltage and gradually increasing it, to test the breakdown voltage.

[0114] Thermal attenuation performance test: The sample was heated at 300°C for 1000 hours, cooled to room temperature, and the resistivity of the sample before and after heating was measured.

[0115] Table 1. Performance test results

[0116]

[0117] According to the comparison of the test results of Example 1 and Comparative Example 1, when the content of silicon dioxide decreases, the thermal expansion coefficient of the high-temperature adhesive is higher than that of the PTC ceramic, resulting in a significant decrease in high-temperature adhesion and thermal attenuation performance.

[0118] According to the comparison of the test results of Example 2 and Comparative Example 2, when the content of silicon dioxide increases, the thermal expansion coefficient of the high-temperature adhesive is lower than that of the PTC ceramic, resulting in a significant decrease in high-temperature adhesion and thermal attenuation performance.

[0119] According to the comparison of the test results of Example 1 and Comparative Example 3, when the silver powder does not meet the conditions specified in the present invention, the breakdown voltage and thermal attenuation performance are reduced.

[0120] According to the comparison of the test results of Example 1 and Comparative Example 4, when the zinc powder does not meet the conditions specified in the present invention, the breakdown voltage and thermal attenuation performance are reduced.

[0121] In summary, the content of silicon dioxide has a great influence on the thermal expansion coefficient of the high-temperature adhesive. Therefore, the method provided by the present invention can effectively control the thermal expansion coefficient of the high-temperature adhesive to match the PTC ceramic, so that the high-temperature adhesive can form a good sintering infiltration with the PTC ceramic body, penetrate into the grain boundary of the ceramic body, melt into one, and form a strong chemical bonding force and mechanical bonding force. In addition, the present invention limits the sphericity and purity of the silver powder and the zinc powder, which can greatly improve the ohmic characteristics of the conductive silver paste.

[0122] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been presented as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. Environmentally friendly ohmic silver paste for PTC heater of new energy vehicles, characterized in that: Calculated by weight, it includes the following components: 40-58 parts of high-purity nano silver powder, 10-20 parts of high-purity nano zinc powder, 5-30 parts of high-temperature binder, 5-20 parts of active additive, 5-15 parts of antioxidant stabilizer, 3-5 parts of dispersing defoaming agent and 10-28 parts of organic carrier; Wherein, the thermal expansion coefficient of the high temperature adhesive matches the thermal expansion coefficient of the ceramic used in the PTC heater; The high-purity nano silver powder has a silver content of 99.95% after burning, a particle size range of 50-200 nm, and a sphericity of ≥80%; The purity of the high-purity nano zinc powder is ≥99.9%, the particle size range is 100-300nm, and the sphericity is ≥85%; The high temperature binder is any one of rare earth oxide modified phosphate, bismuthate, vanadate heat-resistant or water-resistant glass systems; The content of silicon dioxide in the high-temperature adhesive is determined according to the thermal expansion coefficient of the ceramic for the PTC heater, specifically including: setting a threshold value of the difference between the thermal expansion coefficient of the high-temperature adhesive and the thermal expansion coefficient of the ceramic for the PTC heater; determining the thermal expansion coefficient of the high-temperature adhesive according to the threshold value and the thermal expansion coefficient of the ceramic for the PTC heater; and then determining the content of silicon dioxide in the high-temperature adhesive by using a genetic algorithm according to the thermal expansion coefficient of the high-temperature adhesive.

2. The environmentally friendly ohmic silver paste for the PTC heater of new energy vehicles according to claim 1, characterized in that: The active additive is an inorganic nanometer semi-metal element single substance, and the nanometer particle size is 50-100nm.

3. The environmentally friendly ohmic silver paste for the PTC heater of new energy vehicles according to claim 1, characterized in that: The antioxidant stabilizer is any one of phthalate, aluminate or zincate.

4. The environmentally friendly ohmic silver paste for the PTC heater of new energy vehicles according to claim 1, characterized in that: The dispersing defoaming agent is any one of lecithin, synthetic phosphate ester or silicone defoaming agent.

5. The method for preparing the environmentally friendly ohmic silver paste for the PTC heater of new energy vehicles according to claims 1 to 4, characterized in that: The steps include: Weigh high-purity nano silver powder, high-purity nano zinc powder and high-temperature binder according to weight proportions and put them into a pot mill, pot mill for 40h to 48h, and then obtain a premixed powder after ultrasonic dispersion and sieving; Active additives, antioxidant stabilizers, dispersing defoaming agents and organic carriers are added to the premixed powder, and the premixed powder is ground through a three-roll mill.

Citation Information

Patent Citations

  • High-potential gradient zinc oxide voltage piezo-resistor material and preparation method thereof

    CN104591726A

  • Mixed slurry for crystalline silicon solar cell

    CN105655007A

  • Zinc oxide pressure-sensitive resistor electrode silver paste with high silver content and preparation method of silver paste

    CN107993740A

  • Method for preparing co-firing system slurry of surface-lead-silver-free electrode for PTC