A method for preparing polyacrylonitrile pre-oxidized fiber

Through the electronically controlled pre-oxidation method and the use of specific compounds, the problems of fiber uniformity and high energy consumption during the pre-oxidation process of polyacrylonitrile-based carbon fiber are solved, the tensile strength and quality of the fiber are significantly improved, and the defects of the carbon fiber structure are reduced. .

CN118653221BActive Publication Date: 2024-10-22HANGZHOU ZHENLANG IMPORT & EXPORT CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411142466.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-22
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The existing pre-oxidation process of polyacrylonitrile-based carbon fiber has problems such as excessive oxidation of the fiber shell, insufficient oxidation of the inner core, high energy consumption, long time consumption and poor quality, resulting in structural defects and mechanical performance limitations of the carbon fiber.

Method used

The electronically controlled pre-oxidation method is used to promote the internal pre-oxidation of the fiber through compounds such as 2-hydroxyethyl methacrylate and guanidine carbonate, combined with the Joule heating effect of current to homogenize the fiber structure, and use triethanolamine stearate salt to prevent adhesion. Shorten the pre-oxidation reaction time.

Benefits of technology

It improves the uniformity and tensile strength of the fiber, reduces the difference in the degree of cyclization reaction between the inner core and the surface layer, saves energy consumption, avoids fiber bonding, and significantly improves the quality and performance of carbon fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a method for preparing polyacrylonitrile preoxidized fiber. The method uses 2-hydroxyethyl methacrylate and an electrically controlled preoxidation reaction mode to suppress the appearance of a skin-core structure and improve fiber uniformity. A guanidine carbonate solution is used to shorten the preoxidation reaction time, and stearic acid triethanolamine salt treatment is used to avoid adhesion during the preoxidation reaction. The multiple effects increase the tensile strength and improve the performance of the polyacrylonitrile preoxidized fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon fiber, and in particular to a method for preparing polyacrylonitrile pre-oxidized fiber. Background Art

[0002] Polyacrylonitrile-based carbon fiber and its composite materials have the characteristics of high strength and light weight. As structural materials, they are increasingly used in the fields of automobiles, sports, aviation, tools and military equipment. The preparation process of polyacrylonitrile-based carbon fiber mainly includes monomer polymerization, spinning curing, pre-oxidation, high-temperature carbonization, surface treatment and other processes.

[0003] During the pre-oxidation process, the linear macromolecular chain undergoes cyclization, oxidation, dehydrogenation and other reactions to form insoluble and infusible fibers with a heat-resistant trapezoidal structure. The spinning process transforms from chain-like organic polymers to inorganic carbon materials with a graphite-like structure. It is a key link in the preparation of carbon fibers and has an important influence on the structure and properties of the final carbon fibers. The pre-oxidation process usually adopts a continuous gradient heating method to make the spinning react in hot air at 180℃~400℃ to achieve the purpose of pre-oxidation. However, the process still has the following problems that need to be solved.

[0004] (1) The pre-oxidation process is usually carried out in a high-temperature oven or furnace, and the heat is radiated from the outside of the fiber to the inside of the fiber, which may cause the fiber shell to be over-oxidized and the fiber core to be under-oxidized, resulting in a skin-core structure with uneven pre-oxidation of the shell and the core. The skin-core structure will be inherited by the subsequent carbonization treatment, increasing the structural defects of the carbon fiber and limiting the improvement of mechanical properties.

[0005] (2) The pre-oxidation process is usually carried out in a high-temperature oven or furnace at a temperature of 180°C to 400°C for 1 to 3 hours. It is energy-intensive and time-consuming, which increases the cost of carbon fiber manufacturing.

[0006] (3) During the pre-oxidation process, due to the high temperature, the fibers are prone to agglomeration, resulting in deterioration of the quality of the carbon fibers.

[0007] Therefore, it is necessary to develop a method for preparing polyacrylonitrile pre-oxidized fibers which improves the uniformity of the fibers and saves energy and time. Summary of the invention

[0008] In order to solve the above problems, the present invention provides a method for preparing polyacrylonitrile pre-oxidized fiber, comprising the following steps:

[0009] Step S1, preparing a spinning solution: acrylonitrile monomer and 2-hydroxyethyl methacrylate are mixed in a molar ratio of 100:0.5 to 100:1 to prepare a mixture 1; acrylamide is added to the mixture 1 so that the molar ratio of acrylamide to acrylonitrile is 1:100 to 2:100 to prepare a mixture 2; polymerization initiators ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid are dissolved in deionized water to prepare a mixture 3; mixture 3 and mixture 2 are mixed in a mass ratio of 2.5:1 to 3.5:1 to obtain a mixture 4, and the temperature is maintained at 55°C to 60°C for reaction for 70 minutes to 80 minutes; sodium oxalate and sodium bicarbonate are dissolved in deionized water in a molar ratio of 1:5 to prepare a mixture 5; mixture 5 is added to mixture 4, and the pH of mixture 4 is adjusted to 5.5 to 6.0;

[0010] The mixture 4 is dehydrated to obtain a mixture 6; deionized water is added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 is 8:1 to 12:1; the mixture is dehydrated again, the filter cake is formed into particles, and dried at 60° C. to 80° C. for 8 hours to 10 hours to obtain a polyacrylonitrile-based copolymer A;

[0011] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 20% to 30%, and carbon nanotubes are added to make the mass concentration of the carbon nanotubes reach 15% to 20% to prepare a spinning solution B;

[0012] Step S2, preparing polyacrylonitrile fiber precursor: using a dimethylacetamide aqueous solution with a mass concentration of 40% to 50% as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C;

[0013] Step S3, preparation of solution 7: dissolving guanidine carbonate, a pre-oxidation reaction promoter, and triethanolamine stearate, an anti-caking agent, in deionized water to obtain solution 7;

[0014] Step S4, pretreating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7 to pretreat the polyacrylonitrile fiber precursor C;

[0015] Step S5, electrically controlled pre-oxidation reaction to prepare polyacrylonitrile pre-oxidized fiber: connect the polyacrylonitrile fiber precursor C to an electric current of 1 mA to 3 mA, promote the pre-oxidation of the polyacrylonitrile fiber precursor C by the Joule heat of the current, and stretch the length by 2% to 5% at the same time. The pre-oxidation reaction time is 0.5 hour to 2 hours to prepare the polyacrylonitrile pre-oxidized fiber D.

[0016] 2-Hydroxyethyl methacrylate promotes the internal pre-oxidation reaction of the fiber, inhibits the appearance of the skin-core structure, and improves the uniformity of the fiber; while improving the uniformity, it also increases the tensile strength and improves the fiber performance. However, excessive 2-hydroxyethyl methacrylate leads to a decrease in tensile properties. The carboxylate group in the hydroxyalkyl unsaturated carboxylic acid ester, at a high temperature of 240°C, the carboxylate part undergoes thermal decomposition and becomes a carboxylic acid group, which can promote the internal pre-oxidation reaction of the fiber, especially the cyclization reaction, making the fiber more uniform inside and outside. On the other hand, the hydroxyl group in the hydroxyalkyl unsaturated carboxylic acid ester can also promote the cyclization reaction. The combined effect of the two aspects promotes the internal pre-oxidation cyclization reaction of the fiber and reduces the reaction difference between the inner core and the surface of the fiber. Unlike methyl acrylate, 2-hydroxyethyl methacrylate has a relatively large steric hindrance, which can control the oxidation reaction, especially the cyclization reaction. Thirdly, compared with methyl acrylate, the hydroxyalkyl unsaturated carboxylic acid ester is richer in oxygen, releases oxygen at high temperature, and promotes the oxidation reaction.

[0017] Traditional pre-oxidation reaction heating mostly uses equipment such as ovens. Heat and oxygen diffuse from the fiber surface to the inner core. Heat and oxygen are both promoting factors of pre-oxidation reaction, which leads to excessive pre-oxidation of the fiber surface, forming a dense trapezoidal structure, which in turn hinders the diffusion of oxygen into the fiber, resulting in a low degree of reaction in the fiber core, forming a skin-core structure. The heat transfer method of the electrically controlled pre-oxidation reaction is just the opposite. After the polyacrylonitrile fiber precursor is connected to the current, the current can cause the Joule heating effect. The Joule heat diffuses from the fiber core to the surface. The surface temperature is low and the core temperature is high, which accelerates the cyclization reaction of the core, thereby reducing the difference in the degree of cyclization between the core and the surface, improving the fiber uniformity, and improving the fiber quality. Increasing the current can increase the Joule heating effect and increase the fiber temperature. The temperature can reach up to 800°C. By controlling the current, the temperature requirements of the pre-oxidation reaction can be met.

[0018] When the current is too high, the fiber temperature is too high and the surface cyclization reaction rate is faster, which cannot play the effect of reducing the difference in the degree of cyclization between the inner core and the surface.

[0019] It can improve the conductivity of polyacrylonitrile fiber and create conditions for electrically controlled pre-oxidation reaction. Polyacrylonitrile-based carbon nanotube fiber can also be used as anti-static clothing raw material.

[0020] The present invention unexpectedly found that the use of guanidine carbonate solution can significantly shorten the pre-oxidation reaction time, while improving the tensile strength without affecting the skin-to-core ratio. The pre-oxidation time is significantly extended by removing the guanidine carbonate solution treatment step. Guanidine carbonate is a promoter of the pre-oxidation reaction. Guanidine ions are charged and contain carbon-nitrogen double bonds. The activity of guanidine ions in accelerating the pre-oxidation reaction may be due to their more perfect D 3h Symmetry, when the imine nitro group is protonated, rapid resonance can be achieved, accelerating the pre-oxidation of polyacrylonitrile fibers.

[0021] After treatment with triethanolamine stearate, there is no bonding in the pre-oxidation reaction, and the tensile strength is high. When the amine salt is heated to 200°C, the triethanolamine stearate decomposes, becomes insoluble in water, covers the fiber surface, and has a very low permeability in the fiber. This characteristic can effectively prevent fiber bonding, because the permeability of triethanolamine stearate in the fiber is very low, and its effect on the tensile strength of the pre-oxidized fiber is very low. After treatment with siloxane, there is no bonding in the pre-oxidation reaction, but the tensile strength is low. Due to the high permeability and residual rate of siloxane in the fiber, the tensile strength is reduced.

[0022] Examples of the comonomer of the carboxylic acid may include acrylic acid, methacrylic acid, ethacrylic acid, itaconic acid, crotonic acid, citric acid, maleic acid, meconic acid or a mixture thereof, and preferably, itaconic acid may be applied. In this case, the effect of further lowering the starting temperature of the oxidation pre-oxidation reaction performed later may be enhanced.

[0023] As a preferred embodiment, the concentrations of the initiators ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid in the mixture 3 are 0.5 mol / L to 0.7 mol / L, 1.8 mol / L to 2.2 mol / L, and 1.6×10 -4 mol / L~2.0×10 -4 mol / L, 0.25 mol / L~0.35mol / L.

[0024] As a preferred solution, in step S2, the diameter of the spinneret during spinning is 20 μm to 250 μm.

[0025] As a preferred embodiment, the mixture 2 also includes itaconic acid.

[0026] As a preferred embodiment, the mixture 2 further includes butyl acrylate.

[0027] As a preferred embodiment, in the solution 7, the mass concentration of guanidine carbonate is 0.1% to 0.2%.

[0028] As a preferred embodiment, in the solution 7, the mass concentration of triethanolamine stearate is 0.5% to 1.0%.

[0029] As a preferred solution, in step S4, the soaking time is 0.5 hour to 1 hour, and the soaking temperature is 40° C. to 60° C.

[0030] The second aspect of the present invention also provides a polyacrylonitrile pre-oxidized fiber, which is made by any of the above methods.

[0031] Through the above technical solutions, the present invention produces the following technical effects:

[0032] (1) 2-Hydroxyethyl methacrylate is introduced into the spinning solution to promote the internal pre-oxidation reaction of the fiber, inhibit the appearance of the skin-core structure, and improve the uniformity of the fiber. While improving the uniformity, the tensile strength is also increased, thereby improving the fiber performance.

[0033] (2) The electric control pre-oxidation reaction method is used to reduce the difference in the degree of cyclization reaction between the inner core and the surface layer, improve the fiber uniformity, and improve the fiber quality. By controlling the current, the temperature requirement of the pre-oxidation reaction is met, and the operation is convenient. The electric control pre-oxidation reaction method directly uses the polyacrylonitrile fiber as a resistor to generate heat, saving electricity; while the electric furnace heating method heats the resistor and then transfers it to the polyacrylonitrile fiber, which has a high energy consumption.

[0034] (3) The use of guanidine carbonate solution can shorten the pre-oxidation reaction time and improve the tensile strength without affecting the skin-core ratio.

[0035] (4) Use triethanolamine stearate salt treatment to avoid bonding caused by pre-oxidation reaction, and the tensile strength is higher. DETAILED DESCRIPTION

[0036] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the applicant first explains the specific research process of the present invention, and then conducts process verification and comparative analysis through specific embodiments and comparative examples.

[0037] Specific research process:

[0038] 1. Effect of hydroxyalkyl unsaturated carboxylic acid ester on pre-oxidation uniformity

[0039] 1.1 Sample preparation test method

[0040] Preparation of test sample 1:

[0041] Step S1: Preparation of spinning solution,

[0042] Acrylonitrile and 2-hydroxyethyl methacrylate are mixed in a molar ratio of 100:0.5 to prepare a mixture 1, and acrylamide is added to the mixture 1 so that the molar ratio of acrylamide to acrylonitrile is 1:100 to prepare a mixture 2;

[0043] The polymerization initiators ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid were dissolved in deionized water to a concentration of 0.5 mol / L, 1.8 mol / L, and 1.6×10 -4 mol / L, 0.25 mol / L, to prepare mixture 3;

[0044] Mixture 3 and mixture 2 were mixed at a mass ratio of 2.5:1 to obtain mixture 4, and the reaction was maintained at 55° C. for 70 minutes;

[0045] dissolving sodium oxalate and sodium bicarbonate in deionized water at a molar ratio of 1:5 to prepare mixture 5; adding mixture 5 to mixture 4 to adjust the pH of mixture 4 to 5.5;

[0046] The mixture 4 was dehydrated to obtain a mixture 6; deionized water was added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 was 8:1; the mixture was dehydrated again, the filter cake was formed into particles, and dried at 60° C. for 8 hours to obtain a polyacrylonitrile-based copolymer A;

[0047] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 20% to prepare a spinning solution B;

[0048] Step S2: using a 40% dimethylacetamide aqueous solution as a coagulation bath, maintaining the temperature at 40° C., spinning the spinning solution by wet spinning to produce polyacrylonitrile fiber precursor C; the spinneret diameter is 250 μm;

[0049] Step S3: preparing solution 7, which is deionized water;

[0050] Step S4: soaking the polyacrylonitrile fiber precursor C in the solution 7 to pretreat the polyacrylonitrile fiber precursor B;

[0051] Step S5: maintaining the temperature at 240° C. for 2 hours in an air atmosphere while stretching the fiber by 2% to pre-oxidize the polyacrylonitrile fiber precursor C to prepare the polyacrylonitrile pre-oxidized fiber D.

[0052] Preparation of test sample 2:

[0053] The molar ratio of acrylonitrile to 2-hydroxyethyl methacrylate was 100:1, and other conditions were consistent with those of test sample 1.

[0054] Preparation of test sample 3:

[0055] The molar ratio of acrylonitrile to 2-hydroxyethyl methacrylate was 100:1.5, and other conditions were consistent with those of test sample 1.

[0056] Preparation of test sample 4:

[0057] The molar ratio of acrylonitrile to 2-hydroxyethyl methacrylate was 100:0, and other conditions were consistent with those of test sample 1.

[0058] Test sample 5 preparation:

[0059] 2-Hydroxyethyl methacrylate was replaced with methyl acrylate, and other conditions were consistent with those of Test Sample 1.

[0060] 1.2 Test items and methods

[0061] The skin-core ratio was determined by optical microscopy: a mixture of epoxy resin and curing agent = 15:2 (mass ratio) was used to embed polyacrylonitrile pre-oxidized fiber D. After curing at 60°C for 2 hours, the fiber was sliced ​​using an EM TRIM2 ultrathin slicer from Leica, Germany. The sample thickness was about 400 nm. The slices were then observed under a BX53M high-power optical microscope from Olympus, Japan, using a 20X objective lens. The optical density values ​​were analyzed using ImageJ software based on the different transmittances of the cortex and core, and the skin-core ratio was calculated using the formula: cortex area of ​​the fiber cross section / total area*100%.

[0062] The methods for measuring tensile strength and fiber breaking elongation are prior art and will not be described in detail here.

[0063] 1.3 Test results and analysis

[0064] 2-Hydroxyethyl methacrylate promotes the pre-oxidation reaction inside the fiber, inhibits the appearance of the skin-core structure, and improves the uniformity of the fiber; while improving the uniformity, it also increases the tensile strength and improves the fiber performance. However, excessive 2-Hydroxyethyl methacrylate leads to a decrease in tensile properties.

[0065] The carboxylate group in the hydroxyalkyl unsaturated carboxylate undergoes thermal decomposition at a high temperature of 240°C to become a carboxylic acid group, which can promote the pre-oxidation reaction inside the fiber, especially the cyclization reaction, making the fiber surface more uniform.

[0066] On the other hand, the hydroxyl group in the hydroxyalkyl unsaturated carboxylic acid ester can also promote the cyclization reaction. Unlike methyl acrylate, 2-hydroxyethyl methacrylate has a relatively large steric hindrance, which can control the pre-oxidation reaction, especially the cyclization reaction. The combined effect of the two aspects promotes the pre-oxidation cyclization reaction inside the fiber and reduces the reaction difference between the fiber core and the surface.

[0067] Thirdly, compared with methyl acrylate, hydroxyalkyl unsaturated carboxylic acid esters are richer in oxygen, releasing oxygen at high temperatures to promote oxidation reactions.

[0068] Table 1 Test results of hydroxyalkyl unsaturated carboxylic acid esters

[0069]

[0070] 2. Study on electronically controlled pre-oxidation reaction

[0071] 2.1 Sample preparation test method

[0072] Preparation of test sample 6:

[0073] The spinning solution B also includes carbon nanotubes, and the mass ratio of acrylonitrile to carbon nanotubes is 6:1; in step S5, the polyacrylonitrile fiber precursor C is connected to an electric current of 1 mA, and a pre-oxidation reaction is performed by an electric control method for 2 hours. The current promotes the pre-oxidation of the polyacrylonitrile fiber precursor B through Joule heat to prepare the polyacrylonitrile pre-oxidized fiber D. Other conditions are consistent with the preparation method of the test sample 1.

[0074] Test sample 7 preparation:

[0075] The spinning solution B also includes carbon nanotubes, and the mass ratio of acrylonitrile to carbon nanotubes is 5:1; in step S5, the polyacrylonitrile fiber precursor C is connected to an electric current of 1 mA, and a pre-oxidation reaction is performed by an electric control method for 2 hours. The current promotes the pre-oxidation of the polyacrylonitrile fiber precursor B through Joule heat to prepare the polyacrylonitrile pre-oxidized fiber D. Other conditions are consistent with the preparation method of the test sample 1.

[0076] Test sample 8 preparation:

[0077] The spinning solution B also includes carbon nanotubes, and the mass ratio of acrylonitrile to carbon nanotubes is 3:1; in step S5, the polyacrylonitrile fiber precursor C is connected to an electric current of 1 mA, and a pre-oxidation reaction is performed by an electric control method for 2 hours. The current promotes the pre-oxidation of the polyacrylonitrile fiber precursor B through Joule heat to prepare the polyacrylonitrile pre-oxidized fiber D. Other conditions are consistent with the preparation method of the test sample 1.

[0078] Test sample 9 preparation:

[0079] In step S5, the polyacrylonitrile fiber precursor C is connected to an electric current of 3 mA, and other conditions are consistent with the preparation method of test sample 6.

[0080] Preparation of test sample 10:

[0081] In step S5, the polyacrylonitrile fiber precursor C is connected to an electric current of 6 mA, and other conditions are consistent with the preparation method of the test sample 6.

[0082] 2.2 Test items and methods

[0083] The determination methods of skin-core ratio, tensile strength and fiber breaking elongation are consistent with those in “1.2 Test Items and Test Methods”.

[0084] The method for measuring fiber conductivity is a prior art and will not be described in detail here.

[0085] 2.3 Test results and analysis

[0086] The test results are shown in the table below.

[0087] Compared with test sample 1, the skin-core structure disappeared after the electric-controlled pre-oxidation reaction in test samples 6 to 9, and the electric-controlled pre-oxidation reaction method effectively inhibited the formation of the skin-core structure. When the current is too high, the fiber temperature is too high and the surface cyclization reaction speed is too fast, which weakens the effect of inhibiting the skin-core structure.

[0088] Traditional pre-oxidation reaction heating mostly uses equipment such as ovens. Heat and oxygen diffuse from the fiber surface to the inner core. Heat and oxygen are both factors that promote pre-oxidation reaction, resulting in excessive pre-oxidation of the fiber surface, forming a dense trapezoidal structure, which in turn hinders the diffusion of oxygen into the fiber, resulting in a low degree of reaction in the fiber core, forming a skin-core structure. The heat transfer method of the electrically controlled pre-oxidation reaction is just the opposite. After the polyacrylonitrile fiber precursor is connected to the current, the current can cause the Joule heating effect. The Joule heat diffuses from the fiber core to the surface. The surface temperature is low and the core temperature is high, which accelerates the cyclization reaction of the core, thereby reducing the difference in the degree of cyclization between the core and the surface, improving the fiber uniformity, and improving the fiber quality. Increasing the current can increase the Joule heating effect and increase the fiber temperature. The temperature can reach up to 800°C. By controlling the current, the temperature requirement of the pre-oxidation reaction can be met. Carbon nanotubes can improve the conductivity of polyacrylonitrile fibers and create conditions for electrically controlled pre-oxidation reactions.

[0089] Table 2 Test results of electronically controlled pre-oxidation reaction

[0090]

[0091] 3. Study on the accelerated pre-oxidation reaction of guanidine carbonate

[0092] 3.1 Sample preparation test method

[0093] Preparation of test sample 11: In step S3, solution 7 is a guanidine carbonate solution with a mass concentration of 0.1% guanidine carbonate. The solution is immersed for 1 hour at a temperature of 40°C. Other conditions are consistent with the preparation method of test sample 6.

[0094] Preparation of test sample 12: In step S5, the reaction time is 1.5 hours, and other conditions are consistent with the preparation method of test sample 11.

[0095] Preparation of test sample 13: In step S5, the reaction time is 1.0 hour, and other conditions are consistent with the preparation method of test sample 11.

[0096] Preparation of test sample 14: In step S5, the reaction time is 0.5 hours, and other conditions are consistent with the preparation method of test sample 11.

[0097] Preparation of test sample 15: In step S5, the reaction time is 0.5 hours, solution 7 is deionized water, and other conditions are consistent with the preparation method of test sample 11.

[0098] 3.2 Detection methods

[0099] The determination methods of skin-core ratio, fiber breaking elongation and tensile strength are consistent with those in “1.2 Test Items and Test Methods”.

[0100] 3.3 Test results and analysis

[0101] The test results are shown in the table below.

[0102] The use of guanidine carbonate solution can significantly shorten the pre-oxidation reaction time, while improving the tensile strength without affecting the skin-core ratio. Removing the guanidine carbonate solution treatment step significantly extends the pre-oxidation time.

[0103] The guanidine cation is charged and contains a carbon-nitrogen double bond. The increased activity of the guanidine ion may be due to its more perfect D 3h Symmetry, therefore, when the imine nitro group is protonated, rapid resonance can be achieved, accelerating the pre-oxidation of polyacrylonitrile fibers.

[0104] Table 3 Guanidine carbonate test results

[0105]

[0106] 4. Study on pre-oxidation reaction of triethanolamine stearate

[0107] 4.1 Sample preparation test method

[0108] Preparation of test sample 16: In step S3, solution 7 contains guanidine carbonate and triethanolamine stearate, the mass concentration of guanidine carbonate is 0.1%, and the mass concentration of triethanolamine stearate is 0.5%. The solution is immersed for 1 hour at a temperature of 40°C. Other conditions are consistent with the preparation method of test sample 13.

[0109] Preparation of test sample 17: In step S3, solution 7 contains guanidine carbonate, siloxane, and polyoxyethylene. The mass concentration of guanidine carbonate is 0.1%, the mass concentration of siloxane is 0.5%, and the mass concentration of polyoxyethylene is 0.5%. The solution is immersed for 1 hour at a temperature of 40°C. Other conditions are consistent with the preparation method of test sample 13.

[0110] Stearic acid triethanolamine salt is synthesized by heating stearic acid, triethanolamine and HCl.

[0111] 3.2 Detection methods

[0112] The determination methods of tensile strength and fiber breaking elongation are consistent with “1.2 Test Items and Test Methods”.

[0113] Statistical fiber bonding rate.

[0114] 3.3 Test results and analysis

[0115] The test results are shown in the table below.

[0116] Comparative analysis with the test results of test sample 13

[0117] After the treatment of triethanolamine stearate salt, there is no bonding in the pre-oxidation reaction, and the tensile strength is high. When the fiber treated with ammonium salt is heated to 200°C, the triethanolamine stearate salt decomposes, becomes insoluble in water, covers the fiber surface, and has a very low permeability in the fiber. This characteristic can effectively prevent fiber bonding, because the permeability of triethanolamine stearate salt in the fiber is very low, and its effect on the tensile strength of the pre-oxidized fiber is very low.

[0118] After siloxane treatment, the pre-oxidation reaction did not cause bonding, but the tensile strength was low. Due to the high permeability and residual rate of siloxane in the fiber, the tensile strength was reduced.

[0119] Table 4 Test results of triethanolamine stearate

[0120]

[0121] Step S1, preparing a spinning solution: acrylonitrile and 2-hydroxyethyl methacrylate are mixed in a molar ratio of 100:0.5 to 100:1 to prepare a mixture 1; acrylamide is added to the mixture 1 so that the molar ratio of acrylamide to acrylonitrile is 1:100 to 2:100 to prepare a mixture 2; ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid as polymerization initiators are dissolved in deionized water so that their concentrations reach 0.5 mol / L to 0.7 mol / L, 1.8 mol / L to 2.2 mol / L, and 1.6×10 -4 mol / L~2.0×10 -4 mol / L, 0.25 mol / L~0.35 mol / L, to prepare mixture 3; mix mixture 3 and mixture 2 at a mass ratio of 2.5:1~3.5:1 to obtain mixture 4, and keep the temperature at 55℃~60℃ for 70 minutes~80 minutes; dissolve sodium oxalate and sodium bicarbonate in deionized water at a molar ratio of 1:5 to prepare mixture 5; add mixture 5 to mixture 4, and adjust the pH of mixture 4 to 5.5~6.0;

[0122] The mixture 4 is dehydrated to obtain a mixture 6; deionized water is added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 is 8:1 to 12:1; the mixture is dehydrated again, the filter cake is formed into particles, and dried at 60° C. to 80° C. for 8 hours to 10 hours to obtain a polyacrylonitrile-based copolymer A;

[0123] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 20% to 30%, and carbon nanotubes are added to make the mass concentration of the carbon nanotubes reach 15% to 20% to prepare a spinning solution B;

[0124] Step S2, spinning to prepare polyacrylonitrile fiber precursor: using a dimethylacetamide aqueous solution with a mass concentration of 40% to 50% as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C; the spinneret diameter is 20 μm to 250 μm;

[0125] Step S3, preparation of solution 7: dissolving guanidine carbonate, a pre-oxidation reaction promoter, and triethanolamine stearate, an anti-caking agent, in deionized water to obtain solution 7; the mass concentration of guanidine carbonate is 0.1% to 0.2%, and the mass concentration of triethanolamine stearate is 0.5% to 1.0%;

[0126] Step S4, pre-treating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7, the soaking time is 0.5 hour to 1 hour, the soaking temperature is 40° C. to 60° C., and the polyacrylonitrile fiber precursor C is pre-treated;

[0127] Step S5, electrically controlled pre-oxidation reaction to prepare polyacrylonitrile pre-oxidized fiber: connect the polyacrylonitrile fiber precursor C to an electric current of 1 mA to 7 mA, promote the pre-oxidation of the polyacrylonitrile fiber precursor C by the Joule heat of the current, and the pre-oxidation reaction time is 0.5 hour to 2 hours to prepare the polyacrylonitrile pre-oxidized fiber D. Example 1

[0128] Step S1, preparing a spinning solution: acrylonitrile and 2-hydroxyethyl methacrylate are mixed in a molar ratio of 100:0.5 to prepare a mixture 1; acrylamide is added to the mixture 1 so that the molar ratio of acrylamide to acrylonitrile is 1:100 to prepare a mixture 2; and a polymerization initiator ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid are dissolved in deionized water to make their concentrations reach 0.5 mol / L, 1.8 mol / L, and 1.6×10 -4 mol / L, 0.25 mol / L, to prepare mixture 3; mixture 3 and mixture 2 were mixed at a mass ratio of 2.5:1 to obtain mixture 4, and the temperature was maintained at 55°C for 70 minutes; sodium oxalate and sodium bicarbonate were dissolved in deionized water at a molar ratio of 1:5 to prepare mixture 5; mixture 5 was added to mixture 4, and the pH of mixture 4 was adjusted to 5.5;

[0129] The mixture 4 was dehydrated to obtain a mixture 6; deionized water was added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 was 8:1; the mixture was dehydrated again, the filter cake was formed into particles, and dried at 60° C. for 8 hours to obtain a polyacrylonitrile-based copolymer A;

[0130] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 20%, and carbon nanotubes are added to make the mass concentration of the carbon nanotubes reach 15% to prepare a spinning solution B;

[0131] Step S2, spinning to prepare polyacrylonitrile fiber precursor: using a 40% dimethylacetamide aqueous solution as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C; the spinneret diameter is 20 μm;

[0132] Step S3, preparation of solution 7: dissolving guanidine carbonate, a pre-oxidation reaction promoter, and triethanolamine stearate, an anti-caking agent, in deionized water to obtain solution 7; the mass concentration of guanidine carbonate is 0.1%, and the mass concentration of triethanolamine stearate is 0.5%;

[0133] Step S4, pre-treating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7 for 0.5 hours at a soaking temperature of 40° C. to pre-treat the polyacrylonitrile fiber precursor C;

[0134] Step S5, electrically controlled pre-oxidation reaction to prepare polyacrylonitrile pre-oxidized fiber: connect the polyacrylonitrile fiber precursor C to an electric current of 1 mA, promote the pre-oxidation of the polyacrylonitrile fiber precursor C through the Joule heat of the current, and stretch the length by 2% at the same time. The pre-oxidation reaction time is 0.5 hours to prepare the polyacrylonitrile pre-oxidized fiber D. Example 2

[0135] Step S1, preparing a spinning solution: acrylonitrile and 2-hydroxyethyl methacrylate are mixed in a molar ratio of 100:0.7 to prepare a mixture 1; acrylamide is added to the mixture 1 so that the molar ratio of acrylamide to acrylonitrile is 1.5:100 to prepare a mixture 2; and a polymerization initiator ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid are dissolved in deionized water to make their concentrations reach 0.6 mol / L, 2.0 mol / L, and 1.8×10 -4 mol / L, 0.30mol / L, to prepare mixture 3; mixture 3 and mixture 2 were mixed at a mass ratio of 3:1 to obtain mixture 4, and the temperature was maintained at 58°C for 75 minutes; sodium oxalate and sodium bicarbonate were dissolved in deionized water at a molar ratio of 1:5 to prepare mixture 5; mixture 5 was added to mixture 4, and the pH of mixture 4 was adjusted to 5.8;

[0136] The mixture 4 was dehydrated to obtain a mixture 6; deionized water was added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 was 10:1; the mixture was dehydrated again, the filter cake was formed into particles, and dried at 70° C. for 9 hours to obtain a polyacrylonitrile-based copolymer A;

[0137] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 25%, and carbon nanotubes are added to make the mass concentration of the carbon nanotubes reach 18% to prepare a spinning solution B;

[0138] Step S2, spinning to prepare polyacrylonitrile fiber precursor: using a 45% mass concentration of dimethylacetamide aqueous solution as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C; the spinneret diameter is 20 μm;

[0139] Step S3, preparation of solution 7: dissolving guanidine carbonate, a pre-oxidation reaction promoter, and triethanolamine stearate, an anti-caking agent, in deionized water to obtain solution 7; the mass concentration of guanidine carbonate is 0.15%, and the mass concentration of triethanolamine stearate is 0.7%;

[0140] Step S4, pre-treating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7 for 0.8 hours at a soaking temperature of 50° C. to pre-treat the polyacrylonitrile fiber precursor C;

[0141] Step S5, electrically controlled pre-oxidation reaction to prepare polyacrylonitrile pre-oxidized fiber: connect the polyacrylonitrile fiber precursor C to an electric current of 2 mA, promote the pre-oxidation of the polyacrylonitrile fiber precursor C through the Joule heat of the current, and stretch the length by 3% at the same time. The pre-oxidation reaction time is 1 hour to prepare the polyacrylonitrile pre-oxidized fiber D. Example 3

[0142] Step S1, preparing a spinning solution: acrylonitrile and 2-hydroxyethyl methacrylate are mixed at a molar ratio of 100:1 to prepare a mixture 1; acrylamide is added to the mixture 1 so that the molar ratio of acrylamide to acrylonitrile is 2:100 to prepare a mixture 2; and a polymerization initiator ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid are dissolved in deionized water to make their concentrations reach 0.7 mol / L, 2.2 mol / L, and 2.0×10 -4 mol / L, 0.35mol / L, to prepare mixture 3; mixture 3 and mixture 2 were mixed at a mass ratio of 3.5:1 to obtain mixture 4, and the temperature was maintained at 60°C for 80 minutes; sodium oxalate and sodium bicarbonate were dissolved in deionized water at a molar ratio of 1:5 to prepare mixture 5; mixture 5 was added to mixture 4, and the pH of mixture 4 was adjusted to 6.0;

[0143] The mixture 4 was dehydrated to obtain a mixture 6; deionized water was added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 was 12:1; the mixture was dehydrated again, the filter cake was formed into particles, and dried at 80° C. for 10 hours to obtain a polyacrylonitrile-based copolymer A;

[0144] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 30%, and carbon nanotubes are added to make the mass concentration of the carbon nanotubes reach 20% to prepare a spinning solution B;

[0145] Step S2, spinning to prepare polyacrylonitrile fiber precursor: using a 50% dimethylacetamide aqueous solution as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C; the spinneret diameter is 20 μm;

[0146] Step S3, preparation of solution 7: dissolving guanidine carbonate, a pre-oxidation reaction promoter, and triethanolamine stearate, an anti-caking agent, in deionized water to obtain solution 7; the mass concentration of guanidine carbonate is 0.2%, and the mass concentration of triethanolamine stearate is 1.0%;

[0147] Step S4, pre-treating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7 for 1 hour at a soaking temperature of 60° C. to pre-treat the polyacrylonitrile fiber precursor C;

[0148] Step S5, electrically controlled pre-oxidation reaction to prepare polyacrylonitrile pre-oxidized fiber: connect the polyacrylonitrile fiber precursor C to an electric current of 3 mA, promote the pre-oxidation of the polyacrylonitrile fiber precursor C through the Joule heat of the current, and stretch the length by 5% at the same time. The pre-oxidation reaction time is 2 hours to prepare the polyacrylonitrile pre-oxidized fiber D.

[0149] Comparative Example 1

[0150] Step S1, preparing spinning solution: adding acrylamide to acrylonitrile to make the molar ratio of acrylamide to acrylonitrile be 1:100 to prepare mixture 2; dissolving polymerization initiators ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid in deionized water to make their concentrations reach 0.5 mol / L, 1.8 mol / L, and 1.6×10 -4 mol / L, 0.25 mol / L, to prepare mixture 3; mixture 3 and mixture 2 were mixed at a mass ratio of 2.5:1 to obtain mixture 4, and the temperature was maintained at 55°C for 70 minutes; sodium oxalate and sodium bicarbonate were dissolved in deionized water at a molar ratio of 1:5 to prepare mixture 5; mixture 5 was added to mixture 4, and the pH of mixture 4 was adjusted to 5.5;

[0151] The mixture 4 was dehydrated to obtain a mixture 6; deionized water was added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 was 8:1; the mixture was dehydrated again, the filter cake was formed into particles, and dried at 60° C. for 8 hours to obtain a polyacrylonitrile-based copolymer A;

[0152] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 20%, thereby preparing a spinning solution B;

[0153] Step S2, spinning to prepare polyacrylonitrile fiber precursor: using a 40% dimethylacetamide aqueous solution as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C; the spinneret diameter is 20 μm;

[0154] Step S3, preparation of solution 7: solution 7 is deionized water;

[0155] Step S4, pre-treating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7 for 0.5 hours at a soaking temperature of 40° C. to pre-treat the polyacrylonitrile fiber precursor C;

[0156] Step S5, heating pre-oxidation reaction to prepare polyacrylonitrile pre-oxidized fiber: in air atmosphere, maintain 240°C for 0.5 hour, and stretch the length by 2% to pre-oxidize the polyacrylonitrile fiber precursor C to prepare polyacrylonitrile pre-oxidized fiber D.

[0157] Comparative Example 2

[0158] Step S1, preparing spinning solution: adding acrylamide to acrylonitrile to make the molar ratio of acrylamide to acrylonitrile be 1.5:100 to prepare mixture 2; dissolving polymerization initiators ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid in deionized water to make their concentrations reach 0.6 mol / L, 2.0 mol / L, and 1.8×10 -4 mol / L, 0.30mol / L, to prepare mixture 3; mixture 3 and mixture 2 were mixed at a mass ratio of 3:1 to obtain mixture 4, and the temperature was maintained at 58°C for 75 minutes; sodium oxalate and sodium bicarbonate were dissolved in deionized water at a molar ratio of 1:5 to prepare mixture 5; mixture 5 was added to mixture 4, and the pH of mixture 4 was adjusted to 5.8;

[0159] The mixture 4 was dehydrated to obtain a mixture 6; deionized water was added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 was 10:1; the mixture was dehydrated again, the filter cake was formed into particles, and dried at 70° C. for 9 hours to obtain a polyacrylonitrile-based copolymer A;

[0160] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 25%, thereby preparing a spinning solution B;

[0161] Step S2, spinning to prepare polyacrylonitrile fiber precursor: using a 45% mass concentration of dimethylacetamide aqueous solution as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C; the spinneret diameter is 20 μm;

[0162] Step S3, preparing solution 7: solution 7 comprises siloxane and polyoxyethylene, wherein the mass concentration of siloxane is 0.5%, and the mass concentration of polyoxyethylene is 0.5%;

[0163] Step S4, pre-treating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7 for 0.8 hours at a soaking temperature of 50° C. to pre-treat the polyacrylonitrile fiber precursor C;

[0164] Step S5, heating pre-oxidation reaction to prepare polyacrylonitrile pre-oxidized fiber: pre-oxidation reaction is carried out at 280° C. in air atmosphere for 1 hour, and the fiber is stretched by 3% to prepare polyacrylonitrile pre-oxidized fiber D.

[0165] Comparative Example 3

[0166] Step S1, preparing spinning solution: adding acrylamide to acrylonitrile to make the molar ratio of acrylamide to acrylonitrile be 2:100 to prepare mixture 2; dissolving polymerization initiators ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid in deionized water to make their concentrations reach 0.7 mol / L, 2.2 mol / L, and 2.0×10 -4 mol / L, 00.35mol / L, to prepare mixture 3; mixture 3 and mixture 2 were mixed at a mass ratio of 3.5:1 to obtain mixture 4, and the temperature was maintained at 60°C for 80 minutes; sodium oxalate and sodium bicarbonate were dissolved in deionized water at a molar ratio of 1:5 to prepare mixture 5; mixture 5 was added to mixture 4, and the pH of mixture 4 was adjusted to 6.0;

[0167] The mixture 4 was dehydrated to obtain a mixture 6; deionized water was added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 was 12:1; the mixture was dehydrated again, the filter cake was formed into particles, and dried at 80° C. for 10 hours to obtain a polyacrylonitrile-based copolymer A;

[0168] The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 30%, and carbon nanotubes are added to make the mass concentration of the carbon nanotubes reach 20% to prepare a spinning solution B;

[0169] Step S2, spinning to prepare polyacrylonitrile fiber precursor: using a 50% dimethylacetamide aqueous solution as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C; the spinneret diameter is 20 μm;

[0170] Step S3, preparation of solution 7: dissolving guanidine carbonate, a pre-oxidation reaction promoter, and triethanolamine stearate, an anti-caking agent, in deionized water to obtain solution 7; the mass concentration of guanidine carbonate is 0.2%, and the mass concentration of triethanolamine stearate is 1.0%;

[0171] Step S4, pre-treating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7 for 1 hour at a soaking temperature of 60° C. to pre-treat the polyacrylonitrile fiber precursor C;

[0172] Step S5, heating pre-oxidation reaction to prepare polyacrylonitrile pre-oxidized fiber: pre-oxidation reaction is carried out at 300°C in air atmosphere for 1 hour, and the length is stretched by 5% at the same time to prepare polyacrylonitrile pre-oxidized fiber D. Pre-oxidation reaction time is 2 hours and the length is stretched by 5% at the same time to prepare polyacrylonitrile pre-oxidized fiber D.

[0173] The skin-core ratio, tensile strength, fiber bonding rate, and fiber elongation at break of the polyacrylonitrile pre-oxidized fibers prepared in Example 1, Example 2, Example 3, and Comparative Example 1, Comparative Example 2, and Comparative Example 3 were measured. The measurement method is consistent with the above-mentioned study. The fiber linear density and limiting oxygen index are both prior art and will not be described in detail here.

[0174] The results show that due to the addition of 2-hydroxyethyl methacrylate in the embodiment of the present invention and the use of an electrically controlled pre-oxidation reaction, the skin-core ratio is significantly higher than that of Comparative Example 3. The technical solution of the present invention is used to improve the degree of oxidation of the inner core, and the skin-core structural difference is eliminated from the surface, thereby further improving the limiting oxygen index, the fiber linear density, the elongation at break, and comprehensively improving the performance and quality of the pre-oxidized fiber.

[0175] Since the embodiment of the present invention adds guanidine carbonate as a pre-oxidation reaction promoter, the pre-oxidation reaction time is significantly shortened. In Comparative Examples 1 and 2, since no promoter is used, under the same conditions, the pre-oxidation reaction is not thorough, the skin-core ratio is low, and the tensile strength is low.

[0176] Since the present invention performs pretreatment with triethanolamine stearate, the fiber bonding phenomenon of the preoxidation reaction is avoided. After siloxane treatment, no bonding occurs in the preoxidation reaction, but the tensile strength is low. Comparative Examples 2 and 3 perform siloxane pretreatment, and since the permeability and residual rate of siloxane in the fiber are high, the tensile strength is reduced.

[0177] Table 5 Comparison of results of examples and comparative examples

[0178]

Claims

1. A method for preparing polyacrylonitrile pre-oxidized fiber, characterized in that: The following steps are involved: Step S1, preparing a spinning solution: acrylonitrile monomer and 2-hydroxyethyl methacrylate are mixed in a molar ratio of 100:0.5 to 100:1 to prepare a mixture 1; acrylamide is added to the mixture 1 so that the molar ratio of acrylamide to acrylonitrile is 1:100 to 2:100 to prepare a mixture 2; polymerization initiators ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid are dissolved in deionized water to prepare a mixture 3; mixture 3 and mixture 2 are mixed in a mass ratio of 2.5:1 to 3.5:1 to obtain a mixture 4, and the temperature is maintained at 55°C to 60°C for reaction for 70 minutes to 80 minutes; sodium oxalate and sodium bicarbonate are dissolved in deionized water in a molar ratio of 1:5 to prepare a mixture 5; mixture 5 is added to mixture 4, and the pH of mixture 4 is adjusted to 5.5 to 6.0; The mixture 4 is dehydrated to obtain a mixture 6; deionized water is added to the mixture 6 and dispersed, and the mass ratio of the deionized water to the mixture 6 is 8:1 to 12:1; the mixture is dehydrated again, the filter cake is formed into particles, and dried at 60° C. to 80° C. for 8 hours to 10 hours to obtain a polyacrylonitrile-based copolymer A; The polyacrylonitrile-based copolymer A is dissolved in dimethylacetamide to make the mass concentration of the polyacrylonitrile-based copolymer A reach 20% to 30%, and carbon nanotubes are added to make the mass concentration of the carbon nanotubes reach 15% to 20% to prepare a spinning solution B; Step S2, spinning to prepare polyacrylonitrile fiber precursor: using a dimethylacetamide aqueous solution with a mass concentration of 40% to 50% as a coagulation bath, spinning the spinning solution by wet spinning to prepare polyacrylonitrile fiber precursor C; Step S3, preparation of solution 7: dissolving guanidine carbonate, a pre-oxidation reaction promoter, and triethanolamine stearate, an anti-caking agent, in deionized water to obtain solution 7; Step S4, pretreating the polyacrylonitrile fiber precursor: soaking the polyacrylonitrile fiber precursor C in the solution 7 to pretreat the polyacrylonitrile fiber precursor C; Step S5, preparing polyacrylonitrile pre-oxidized fiber by electrically controlled pre-oxidation reaction: connecting the polyacrylonitrile fiber precursor C to an electric current of 1 mA to 3 mA, promoting the pre-oxidation of the polyacrylonitrile fiber precursor C by the Joule heat of the current, and stretching the length by 2% to 5% at the same time, and the pre-oxidation reaction time is 0.5 hour to 2 hours to prepare the polyacrylonitrile pre-oxidized fiber.

2. The preparation method according to claim 1, characterized in that The concentrations of the initiators ammonium persulfate, ammonium bisulfite, ferrous sulfate, and sulfuric acid in mixture 3 are 0.5 mol / L to 0.7 mol / L, 1.8 mol / L to 2.2 mol / L, and 1.6×10 -4 mol / L~2.0×10 -4 mol / L, 0.25 mol / L~0.35mol / L.

3. The preparation method according to claim 2, characterized in that: In step S2, the diameter of the spinneret during spinning is 20 μm to 250 μm.

4. The preparation method according to claim 3, characterized in that: Mixture 2 also included itaconic acid.

5. The preparation method according to claim 4, characterized in that: Mixture 2 also included butyl acrylate.

6. The preparation method according to claim 5, characterized in that: In solution 7, the mass concentration of guanidine carbonate is 0.1% to 0.2%.

7. The preparation method according to claim 6, characterized in that: In solution 7, the mass concentration of stearic acid triethanolamine salt is 0.5% to 1.0%.

8. The preparation method according to claim 7, characterized in that: In step S4, the soaking time is 0.5 hour to 1 hour, and the soaking temperature is 40° C. to 60° C.

9. A polyacrylonitrile pre-oxidized fiber, characterized in that: The polyacrylonitrile pre-oxidized fiber is prepared by the preparation method described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Polyacrylonitrile-based carbon fiber precursor polymer and preparation method thereof, and polyacrylonitrile-based carbon fiber and preparation method thereof

    CN110305247A

  • Polyacrylonitrile-based carbon fiber precursor pre-oxidation method

    CN111560666A

  • Microwave pre-oxidation technology for electric-control-type polyacrylonitrile protofilament

    CN111691012A

  • Polyacrylonitrile fiber precursor rapid pre-oxidation method

    CN112553711A

  • Process for producing carbon fiber

    US4735693A