Multilayer nanonetwork interlaced composite bio-based electrochemical sensor and preparation method and application thereof

By constructing a nanosilver network structure and multi-wall carbon nanotubes on the carbonized bamboo sheet substrate to form a bio-based electrochemical sensor with multi-layer nanonetwork interlaced composite, the problem of non-degradable and insufficient environmental protection of traditional electrochemical sensor substrate materials is solved. , realizes high sensitivity formaldehyde detection, conforms to the development trend of environmental protection and is suitable for gaseous detection.

CN118655195BActive Publication Date: 2024-11-26DALIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411147003.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing electrochemical sensor substrate materials are non-degradable and have insufficient environmental protection. The sensor performance is affected by the surface structure of the substrate material, making it difficult to achieve environmentally friendly, low-cost and high-performance detection effects, especially in formaldehyde detection.

Method used

Carbonized bamboo sheets are used as the substrate material, and nanosilver network structure is constructed through drop-sink-drop technology to recombine with multi-wall carbon nanotubes to form a bio-based electrochemical sensor with multi-layer nanonetwork interlaced composite, using nanosilver and carbon nanotubes. Synergistically improves detection performance.

Benefits of technology

It realizes green, environmentally friendly, low-cost high-sensitivity formaldehyde detection. The material is non-toxic and pollution-free, conforms to the development trend of environmental protection, and is easy to produce on a large scale, suitable for gaseous detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118655195B_ABST
    Figure CN118655195B_ABST
Patent Text Reader

Abstract

The present invention discloses a bio-based electrochemical sensor with a multi-layer nano-network interlaced composite, a preparation method and an application thereof. The present invention is based on a carbonized bamboo piece, and a network-like nano-silver is electrochemically deposited on the surface of the carbonized bamboo piece after silver nanowires are compounded thereon, and the electrochemical sensor is combined with multi-walled carbon nanotubes as a base layer and a nano-network active layer. The drip-sink-drop technology of the present invention can realize the multi-layer preparation of nano-materials with different morphologies, and realize the organic fusion between layers. Through the synergistic effect of multi-morphology and multi-layer nano, the electrochemical catalytic oxidation performance of the sensor on the detected substance is promoted. The carbonized bamboo piece substrate has a hierarchical porous structure, and the electrochemically deposited network-like nano-silver and multi-walled carbon nanotubes construct a nano-network structure to produce a synergistic effect, which promotes electrochemical catalytic oxidation. Therefore, the present invention provides a bio-based electrochemical sensor with a multi-layer nano-network interlaced composite with excellent comprehensive performance, a preparation method and an application thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of bio-based electronic materials and the field of sensors, and in particular to a bio-based electrochemical sensor with a nano-silver network structure enhanced by using a biomass carbonized bamboo chip substrate as well as a preparation method and application thereof. Background Art

[0002] In recent years, electrochemical sensors have shown great application potential in the fields of chemistry, environmental science, materials science, etc. due to their advantages such as strong selectivity, high sensitivity and wide detection range. The base material of the electrochemical sensor and the functional nanomaterials composited on the base are its key components and determine the performance of the sensor. Currently, common electrochemical sensor base materials include inorganic carbon materials, metal materials and organic polymer materials, all of which are non-degradable materials and their environmental friendliness needs to be improved. In addition, the surface structure of the base material can affect its composite mechanism with the functional nanomaterials and thus affect the performance of the sensor. Therefore, the research and development of environmentally friendly, low-cost and good-performance electrochemical sensor materials has certain research value and practical significance, especially in the detection of formaldehyde.

[0003] At present, electrochemical sensors are mainly composed of two parts: electrode substrate and electrochemical modification material. Therefore, electrochemical sensors also mainly improve the sensitivity of electrochemical detection by regulating the microscopic morphology of nanostructures and selecting appropriate supporting substrates. In addition, with the reduction of fossil fuels, the use of sustainable materials to develop environmentally friendly electrochemical sensors has gradually become the latest trend.

[0004] As a renewable energy source with great appeal, biomass is gradually gaining more social attention due to its low cost, environmental friendliness and rich heteroatom content. In addition, it has great potential as a substitute for fossil fuels. According to some reports on biomass, some biomass has become the best precursor for preparing carbon-based electrode materials. For example, biomass carbon sources include cherry pits, bamboo, corn cobs, chestnut shells, acorn shells, pecan shells, grape buds, wine lees, coconut shells, lotus stems and palms, which have been proven to be promising electrode materials.

[0005] Electrochemical deposition is an effective method for the controlled preparation of nanostructures with special morphologies on conductive substrates. Electrochemical deposition mainly refers to adding target product ions to an electrolyte solution, and then applying a potential to the substrate material to cause the target product ions to undergo oxidation or reduction reactions, thereby obtaining the desired product at the anode or cathode. Electrodeposition has the advantages of being simple, low-cost and environmentally friendly, and nanostructures with different morphologies can be obtained by adjusting experimental parameters.

[0006] Silver nanoparticles are often more stable, non-toxic, biocompatible, antibacterial, and exhibit high conductivity and good electrocatalytic activity. Carbon nanotubes also play an important role in electrochemical sensors due to their high specific surface area and high catalytic activity. Therefore, using silver nanoparticles and carbon nanotubes as nano-modified materials for electrochemical sensors and utilizing their respective advantages to synergistically exert their respective advantages has a strong advantage in the electrochemical catalytic oxidation of formaldehyde. Summary of the invention

[0007] Based on the above, the present invention provides a method for preparing a bio-based electrochemical sensor with a multi-layer nano-network interlaced composite prepared by a drop-sink-drop technique, which is green and environmentally friendly, has a wide source of raw materials, is simple to prepare, has low cost, and is easy to mass produce. The present invention uses carbonized bamboo chips as the base material, creatively constructs a nano-network structure by a silver-silver composite method, and reinforces the network structure with a multi-walled carbon nanotube composite, effectively utilizes the active sites of nano-silver to composite with the functional oxygen-containing groups of carbonized bamboo chips and multi-walled carbon nanotubes, and drip coating and electrochemical deposition can prepare nanostructures with different morphologies. The drop-sink-drop technique can realize the multi-layer preparation of nanomaterials with different morphologies and realize the organic fusion between layers. Through the synergistic effect of multi-morphology and multi-layer nanostructures, the electrochemical catalytic oxidation performance of the sensor to the detected substance is promoted, and the bio-based electrochemical sensor with a nano-silver network structure enhanced by a carbonized bamboo chip substrate can be prepared. The materials used are green, non-toxic, harmless, and pollution-free, which conforms to the development trend of green environmental protection and embodies an environmentally friendly strategy.

[0008] The multi-layer nano-network interlaced composite bio-based electrochemical sensor prepared by the drop-sink-drop technology described in the present invention is an electrochemical sensor based on carbonized bamboo pieces, which are composited with silver nanowires on the surface and then network-like nanosilver (bn-Ag) is deposited using electrochemical deposition technology, and combined with multi-walled carbon nanotubes (MWNT) as a base layer and a nano-network active layer.

[0009] The primary purpose of the present invention is to claim protection for a bio-based electrochemical sensor with a multi-layer nano-network interlaced composite, which has a carbonized bamboo substrate and a functional nano-material layer attached to its surface, wherein the nano-material layer is a composite of silver nano-wires, nano-silver and carbon nano-tubes.

[0010] The second object of the present invention is to claim a method for preparing a multi-layer nano-network interlaced composite bio-based electrochemical sensor, comprising the following steps:

[0011] (1) Preparation of sensor substrate material: The cut bamboo pieces were ultrasonically treated in deionized water, acetone solution, and anhydrous ethanol respectively. Finally, the cleaned bamboo pieces were taken out and dried, and then carbonized. Finally, after cooling down, the bamboo pieces were taken out and placed in a sealed bag for later use.

[0012] (2) Preparation of silver nanowire ethanol solution: preparing a uniform silver nanowire ethanol solution;

[0013] (3) Drip coating: The dispersed silver nanowire ethanol solution is evenly dripped onto the carbonized bamboo substrate. Ethanol can promote the uniform dispersion of silver nanowires. In addition, ethanol has surface hydrophilicity and can better combine with the silver nanowires and the bamboo surface. The purpose of drip coating silver nanowires here is to improve the conductivity of the carbonized bamboo substrate so as to facilitate the subsequent electrodeposition of silver nanowires.

[0014] (4) Preparation of AgNO3 and NaNO3 mixed solution: prepare a uniform AgNO3 and NaNO3 mixed solution;

[0015] (5) Electrochemical deposition: The carbonized bamboo strips coated with silver nanowires are then used as working electrodes, a mixed solution of AgNO3 and NaNO3 is used as a deposition electrolyte solution, a mercurous sulfate electrode is used as a reference electrode, and a platinum electrode is used as a counter electrode. The nanosilver is deposited on the substrate surface using a constant potential deposition method, thus obtaining a nanosilver carbonized bamboo strip electrode. This deposition operation is repeated, and finally dried;

[0016] (6) Preparation of carbon nanotube ethanol solution: preparing a uniform carbon nanotube ethanol solution;

[0017] (7) Construction of bio-based electrochemical sensor: The dispersed carbon nanotube ethanol solution is evenly dropped onto the carbonized bamboo substrate material to make the carbon nanotubes and the network-like nanosilver composite;

[0018] The nanosilver carbonized bamboo substrate material with electrochemically deposited nanosilver and drop-coated carbon nanotubes is a bio-based electrochemical sensor based on the carbonized bamboo substrate.

[0019] Furthermore, the step (1) is specifically as follows: sensor substrate material preparation: cutting bamboo pieces into specific specifications, then placing the cut bamboo pieces in deionized water for ultrasonic treatment, then drying the water on the surface of the bamboo pieces and placing them in an acetone solution for ultrasonic treatment, then taking the bamboo pieces out of the acetone solution and leaving them until the acetone on the surface evaporates, then placing the bamboo pieces in anhydrous ethanol for ultrasonic cleaning, finally taking out the cleaned bamboo pieces and placing them in a vacuum drying oven at 45°C for drying, followed by carbonization of the bamboo pieces, placing the cleaned bamboo pieces evenly on a high-temperature resistant alumina ceramic sheet and placing them in a muffle furnace, introducing nitrogen to ensure that the carbonization is carried out in a nitrogen atmosphere at high temperature, and finally taking them out and placing them in a sealed bag for standby use after cooling.

[0020] Furthermore, the bamboo pieces in step (1) have a specification range of: 1-10 cm in length, 0.1-10 cm in width, and 0.01-4 cm in thickness; a high temperature range of: 300° C.-450° C.; and a carbonization time range of 20-60 min.

[0021] Furthermore, the concentration range of the prepared silver nanowire ethanol solution in step (2) is 0.1 mg / mL-5 mg / mL.

[0022] Furthermore, the drip coating step in step (3) can be repeated for multiple layers, with a total number of drip coating layers of 1-14; the total amount of solution dripped in each layer ranges from 350 to 500 μL.

[0023] Furthermore, the mixed solution of AgNO3 and NaNO3 in step (4) is a mixture of 0.01-0.1 mol / L AgNO3 and 0.1-1.0 mol / L NaNO3.

[0024] Furthermore, in step (5), the potential range of the constant potential deposition method is -1-0 V; the deposition time range is 800-3000 s; the repeated deposition operation range is 1-6 times. The vacuum drying oven temperature is 45°C.

[0025] Furthermore, the concentration range of the prepared carbon nanotube ethanol solution in step (6) is 0.1 mg / mL-5 mg / mL.

[0026] Furthermore, the drip coating step in step (7) can be repeated for multiple layers, with a total number of drip coating layers of 1-14 layers; the total amount of each layer dripped ranges from 350 to 500 μL.

[0027] The present invention also claims to protect the application of a multi-layer nano-network interlaced composite bio-based electrochemical sensor for gas detection, especially for detecting formaldehyde.

[0028] The significant advantages of the present invention compared with the prior art are:

[0029] 1) The material selection is novel. The present invention uses carbonized bamboo chips as the base material, which has significant advantages such as environmentally friendly production, non-toxicity and pollution-free emissions. The bamboo chip base exhibits a fine hierarchical porous structure, including a large number of micropores and several mesopores, which is conducive to the realization of an efficient electron transfer process. The bamboo chips can be effectively removed from the non-target components inside by high-temperature carbonization treatment, thereby improving the purity of the material. The natural porous structure of the carbonized bamboo chips provides abundant active sites for the nanocomposite materials, and further uses electrochemical deposition technology to uniformly cover the surface with a network-like nanosilver layer. In addition, the carbonized bamboo chips are rich in oxygen-containing functional groups, which can produce strong bonding with nanosilver, thereby optimizing the attachment and distribution of nanosilver on the surface of the bamboo chips.

[0030] 2) The network-like nanosilver structure obtained by electrochemical deposition in the present invention is unique, which not only increases the active surface area of ​​the material, but also promotes the synergistic effect inside the nanocomposite material through its network structure, thereby improving the response sensitivity of the sensor. The sensor prepared by the present invention has a good response to liquid and is particularly suitable for the detection of formaldehyde.

[0031] 3) The "drop-sink-drop" technology used in the present invention is an advanced method for preparing multilayer nanomaterials, which can achieve precise stacking of nanomaterials of different forms and form a tight and orderly combination between layers. This method has the characteristics of simple operation, environmental friendliness, low cost, etc., and is easy to achieve large-scale production, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a flow chart of the preparation of the electrochemical sensor according to an embodiment of the present invention;

[0033] Figure 2 is a scanning electron microscope photograph of the surface of the carbonized bamboo chip substrate according to the embodiment of the present invention;

[0034] Figure 3 is a scanning electron microscope photograph of the electrochemical sensor described in the embodiment of the present invention;

[0035] Figure 4 is an XRD diffraction pattern of an electrochemical sensor tested in the present invention;

[0036] Figure 5 are the reaction kinetics curve and the reaction kinetics linear curve of the electrochemical sensor tested by the present invention; wherein, Figure 5 a is the reaction kinetics curve of the electrochemical sensor; Figure 5 b is the linear curve of the electrochemical sensor;

[0037] Figure 6 The present invention is an electrochemical impedance curve of the electrochemical sensor tested;

[0038] Figure 7 : are cyclic voltammetry curves and cyclic voltammetry linear curves of formaldehyde at different concentrations tested in the embodiment of the present invention; wherein, Figure 7 a is the cyclic voltammetry curve; Figure 7 b is the cyclic voltammetry linear curve. DETAILED DESCRIPTION

[0039] In order to more clearly illustrate the purpose, technical solutions and advantages of the present disclosure, the embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings. It should be understood that the description of the embodiments below is intended to explain and illustrate the overall concept of the present invention, and should not be understood as a limitation of the present invention. For the sake of clarity, the drawings are not necessarily drawn to scale, and some well-known components and structures may be omitted in the drawings. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can be obtained from commercial channels. Bamboo chips, silver nanowires and carbon nanotubes were purchased directly on the market.

[0040] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", etc., are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0041] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood in specific circumstances.

[0042] The bio-based electrochemical sensor comprises a carbonized bamboo sheet substrate and a functional nanomaterial layer attached to the surface thereof, wherein the nanomaterial layer is composited with silver nanowires, nanosilver and carbon nanotubes. A method for preparing a bio-based electrochemical sensor with a nanosilver network structure enhanced based on a carbonized bamboo sheet substrate provided by an embodiment of the present invention comprises the following steps:

[0043] The first step is to make the sensor base material: cut the bamboo strips into specific specifications, then put the cut bamboo strips into deionized water for ultrasonic treatment, then absorb the water on the surface of the bamboo strips and put them into acetone solution for ultrasonic treatment, then take out the bamboo strips from the acetone solution and place them until the acetone on the surface evaporates, then put the bamboo strips into anhydrous ethanol for ultrasonic cleaning, finally take out the cleaned bamboo strips and put them into a vacuum drying oven at 45°C for drying, then carbonize the bamboo strips, evenly place the cleaned bamboo strips on the high-temperature resistant alumina ceramic sheets and put them into a muffle furnace, introduce nitrogen to ensure that the carbonization is carried out in a nitrogen atmosphere, and carbonize at a high temperature of 300-450°C for 20-60 minutes, finally take out the carbonized bamboo strips and place them in a sealed bag for standby use.

[0044] The second step is the preparation of silver nanowire ethanol solution: 5 mg / mL silver nanowires (AgNWs) are diluted with anhydrous ethanol, 80-4000 μL of the silver nanowire solution is transferred into a 5 mL centrifuge tube with a pipette, and then 0-3920 μL of anhydrous ethanol is added to the centrifuge tube to prepare a 0.1-5 mg / mL anhydrous ethanol silver nanowire solution. After preparation, ultrasonicate for 20-30 minutes to fully disperse the silver nanowires in the anhydrous ethanol and stabilize it into a uniform solution.

[0045] The third step is drop coating: the dispersed silver nanowire ethanol solution is evenly drop coated on the cut carbonized bamboo chip substrate material, and 350-500 μL of uniform and stable silver nanowire solution is transferred with a pipette and evenly drop coated on the dried carbonized bamboo chip substrate material, and placed in a vacuum drying oven at 45°C for drying. After drying for 4 hours, it is taken out. At this time, a layer of silver nanowire solution with a concentration of 0.1-5 mg / mL has been drop coated on the carbonized bamboo chip substrate material. Repeat this drop coating step to obtain a carbonized bamboo chip drop coated with silver nanowire ethanol solution. This step can be drop coated 1-14 layers. After each layer is dropped, it is placed in a vacuum drying oven for drying for 4 hours before dropping another layer. The role of drop coating of silver nanowires here is to improve the conductivity of the carbonized bamboo chip substrate for subsequent electrodeposition to prepare silver nanowires.

[0046] The fourth step is the preparation of the mixed solution of AgNO3 and NaNO3: weigh 0.849-8.49g of AgNO3 and 4.25-42.25g of NaNO3 into a 500mL volumetric flask, and then add deionized water to the scale line to prepare a 0.01-0.1mol / L AgNO3 and 0.1-1.0mol / L NaNO3 mixed solution. The prepared mixed solution is then ultrasonicated for 20 minutes to fully disperse AgNO3 and NaNO3 in the deionized water and stabilize into a uniform solution.

[0047] Step 5, electrochemical deposition: Use the carbonized bamboo strips after drop coating with silver nanowires as the working electrode, the mixed solution of AgNO3 and NaNO3 as the deposition electrolyte solution, the mercurous sulfate electrode as the reference electrode, and the platinum electrode as the counter electrode. Use the constant potential deposition method to apply a potential of -1-0V, set the deposition time to 800-3000s to deposit nanosilver on the substrate surface. Repeat this deposition operation 1-6 times, and place it in a vacuum drying oven to dry at 45°C.

[0048] Step 6. Preparation of carbon nanotube ethanol solution: weigh 0.0004-0.02g of carboxylated multi-walled carbon nanotubes (CNT) into a 5mL centrifuge tube, and then add 4mL of anhydrous ethanol to prepare a 0.1mg / mL-5mg / mL carboxylated multi-walled carbon nanotube ethanol solution. After preparation, ultrasonicate for 40 minutes to fully disperse the carbon nanotubes in the ethanol and stabilize it into a uniform solution.

[0049] Step 7, drop coating: Alternately and evenly drop the dispersed carbon nanotube ethanol solution onto the carbonized bamboo chip substrate material on which nanosilver has been deposited, and use a pipette to transfer 350-500 μL of a uniform and stable 0.1 mg / mL-5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution and evenly drop it on it. At this time, a layer of 0.5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution has been drop-coated on the carbonized bamboo chip substrate material. Repeat this drop coating step to obtain a carbonized bamboo chip of carboxylated multi-walled carbon nanotube ethanol solution. This step can be drop-coated 1-14 layers. After each layer is dropped, it is placed in a vacuum drying oven to dry for 3-4 hours and then drop another layer to obtain a nanosilver composite carbon nanotube carbonized bamboo chip electrode. The carbon nanotubes and nanosilver after drop coating produce a synergistic effect to promote the electrochemical catalytic oxidation and response of formaldehyde. The bamboo chip substrate has a hierarchical porous structure with numerous micropores and several mesopores, which can achieve high-speed electron transfer and is expected to obtain a highly sensitive electrochemical sensor.

[0050] Example 1 Sensor Sample Preparation

[0051] The preparation process of sensor samples is as follows Figure 1 shown.

[0052] (1) Cut the bamboo strips into 4 cm × 1 cm × 1 cm specifications, then put the cut bamboo strips into deionized water for ultrasonic treatment for 10 min, then absorb the water on the surface of the bamboo strips and put them into acetone solution for ultrasonic treatment for 10 min, then take out the bamboo strips from the acetone solution and leave them until the acetone on the surface evaporates, then put the bamboo strips into anhydrous ethanol for ultrasonic cleaning for 10 min, finally take out the cleaned bamboo strips and put them into a vacuum drying oven at 45 °C for drying, then carbonize the bamboo strips, evenly place the cleaned bamboo strips on a high-temperature resistant alumina ceramic sheet and put them into a muffle furnace, introduce nitrogen to ensure that the carbonization is in a nitrogen atmosphere, and carbonize at a temperature of 330 °C for 20 min, finally take them out and put them into a sealed bag for use.

[0053] (2) Use a pipette to transfer 600 μL of 5 mg / mL silver nanowire solution to a 5 mL microcentrifuge tube, then use a pipette to transfer 3400 μL of anhydrous ethanol to the same microcentrifuge tube, and then ultrasonicate for 30 min to prepare 4 mL of 0.75 mg / mL silver nanowire solution.

[0054] (3) Use a pipette to transfer 400 μL of 0.75 mg / mL silver nanowire ethanol solution from a microcentrifuge tube and evenly apply it on the dry carbonized bamboo substrate. Then place it in a vacuum drying oven and dry it for 4 hours. The sample is coated with one layer. At this point, a layer of 1 mg / mL silver nanowire solution has been applied to the carbonized bamboo substrate.

[0055] (4) Weigh 0.849 g of AgNO3 and 4.25 g of NaNO3 into a 500 mL volumetric flask, then add deionized water to the mark. After preparation, ultrasonicate for 20 min to fully disperse AgNO3 and NaNO3 in the deionized water to prepare a mixed solution of 0.01 mol / L AgNO3 and 0.1 mol / L NaNO3.

[0056] The prepared mixed solution was ultrasonicated for 20 minutes to fully disperse AgNO3 and NaNO3 in deionized water.

[0057] The carbonized bamboo strips after drop coating with silver nanowires were used as working electrodes, the mixed solution of AgNO3 and NaNO3 was used as the deposition electrolyte solution, the mercurous sulfate electrode was used as the reference electrode, and the platinum electrode was used as the counter electrode. The potential was applied to -1V by the constant potential deposition method, and the deposition time was set to 800s to deposit the nanosilver on the substrate surface. This deposition operation was repeated twice, and the substrate was placed in a vacuum drying oven and dried at 45°C.

[0058] Weigh 0.002 g of carboxylated multi-walled carbon nanotubes (CNT) into a 5 mL centrifuge tube, and then add 4 mL of anhydrous ethanol to prepare a 0.5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution. After preparation, ultrasonicate for 40 minutes to fully disperse the carbon nanotubes in the ethanol to prepare a 0.5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution.

[0059] Alternately and evenly drop dispersed carbon nanotube ethanol solution onto the carbonized bamboo substrate material with deposited nanosilver, and use a pipette to transfer 400 μL of uniform and stable 0.5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution and evenly drop it onto it. At this time, a layer of 0.5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution has been drop-coated onto the carbonized bamboo substrate material. The nanosilver composite carbon nanotube carbonized bamboo substrate material is obtained. The microstructure of this sample is shown in the attached figure. Figure 2 shown. Figure 2 The microstructure of the carbonized bamboo substrate is Figure 2 It can be seen that the carbonized bamboo substrate has a hierarchical porous structure with numerous micropores and several mesopores. Figure 3 This is a scanning electron microscope photo of the electrochemical sensor described in an embodiment of the present invention. The electrochemically deposited network-like nanosilver has a unique network-like morphology and can provide more active sites. Figure 3 It can be seen that nanosilver and carbon nanotubes interpenetrate and cross-link to form a network. This structure is conducive to the synergistic effect of the two nanomaterials, thereby promoting electrochemical response and sensitivity.

[0060] Example 2 Sensor sample preparation

[0061] The preparation process of sensor samples is as follows Figure 1 shown.

[0062] The bamboo strips were cut into a size of 5cm×2cm×0.1cm, and then the cut bamboo strips were placed in deionized water for ultrasonic treatment for 10 minutes. After the water on the surface of the bamboo strips was absorbed, they were placed in an acetone solution for ultrasonic treatment for 10 minutes. Then the bamboo strips were taken out from the acetone solution and placed until the acetone on the surface evaporated. Then the bamboo strips were placed in anhydrous ethanol for ultrasonic cleaning for 10 minutes. Finally, the cleaned bamboo strips were taken out and placed in a vacuum drying oven at 45°C for drying. Then the bamboo strips were carbonized. The cleaned bamboo strips were evenly placed on high-temperature resistant alumina ceramic sheets and placed in a muffle furnace. Nitrogen was introduced to ensure that the carbonization was carried out in a nitrogen atmosphere. The carbonization was carried out at a temperature of 360°C for 30 minutes. Finally, the bamboo strips were taken out and placed in a sealed bag for later use.

[0063] Use a pipette to transfer 800 μL of a 5 mg / mL silver nanowire solution to a 5 mL microcentrifuge tube, and then use a pipette to transfer 3200 μL of anhydrous ethanol to the same microcentrifuge tube, and then ultrasonicate for 30 minutes to prepare 4 mL of a 1 mg / mL silver nanowire solution.

[0064] 350 μL of 1 mg / mL silver nanowire ethanol solution was evenly applied to the dried carbonized bamboo substrate using a pipette from a microcentrifuge tube, and then placed in a vacuum drying oven for 4 hours to coat the sample with one layer. Repeat this coating step once, so that two layers of 1 mg / mL silver nanowire solution were coated on the carbonized bamboo substrate.

[0065] Weigh 1.698g of AgNO3 and 8.5g of NaNO3 into a 500mL volumetric flask, then add deionized water to the scale line. After preparation, ultrasonicate for 20min to fully disperse AgNO3 and NaNO3 in the deionized water to prepare a mixed solution of 0.02mol / L AgNO3 and 0.2mol / L NaNO3. After preparation, ultrasonicate for 20min to fully disperse AgNO3 and NaNO3 in the deionized water.

[0066] The carbonized bamboo strips after drop coating with silver nanowires were used as working electrodes, the mixed solution of AgNO3 and NaNO3 was used as the deposition electrolyte solution, the mercurous sulfate electrode was used as the reference electrode, and the platinum electrode was used as the counter electrode. The potential was applied to -0.6V by constant potential deposition method, and the deposition time was set to 1000s to deposit nanosilver on the substrate surface. This deposition operation was repeated 3 times and placed in a vacuum drying oven to dry at 45°C.

[0067] Weigh 0.004 g of carboxylated multi-walled carbon nanotubes (CNTs) into a 5 mL centrifuge tube, and then add 4 mL of anhydrous ethanol to prepare a 1 mg / mL carboxylated multi-walled carbon nanotube ethanol solution. After preparation, ultrasonicate for 40 minutes to fully disperse the carbon nanotubes in the ethanol to prepare a 1 mg / mL carboxylated multi-walled carbon nanotube ethanol solution.

[0068] The dispersed carbon nanotube ethanol solution was alternately and evenly dripped onto the carbonized bamboo substrate material on which nanosilver had been deposited. 350 μL of a uniform and stable 1 mg / mL carboxylated multi-walled carbon nanotube ethanol solution was transferred with a pipette and evenly dripped on it. At this time, one layer of 1 mg / mL carboxylated multi-walled carbon nanotube ethanol solution had been dripped on the carbonized bamboo substrate material. This dripping step was repeated once, i.e., two layers of carboxylated multi-walled carbon nanotube ethanol solution were dripped.

[0069] The present invention has carried out XRD characterization on the sensor, and the test results are as follows Figure 4 It is obvious that there are four diffraction peaks at 38.08°, 44.3°, 64.12° and 77.3° in the spectrum, which correspond to Ag(111), Ag(200), Ag(220) and Ag(311) planes respectively. This also proves that nanosilver is successfully deposited on the carbonized bamboo substrate. In addition to a series of diffraction peaks of nano-Ag, a wide diffraction peak can be observed at about 21.8°, which is the diffraction peak corresponding to the C(202) plane CNT. This also proves the successful preparation of the sensor and the successful construction of the network structure of the network-like nanosilver layer and multi-walled carbon nanotubes, which is consistent with the results of the scanning electron microscope, that is, a nanosilver composite carbon nanotube carbonized bamboo electrode is obtained.

[0070] Example 3 Sensor Sample Preparation

[0071] The preparation process of sensor samples is as follows Figure 1 shown.

[0072] The bamboo strips were cut into a size of 6cm×3cm×2cm, and then the cut bamboo strips were placed in deionized water for ultrasonic treatment for 10 minutes. After the water on the surface of the bamboo strips was absorbed, the bamboo strips were placed in an acetone solution for ultrasonic treatment for 10 minutes. Then the bamboo strips were taken out from the acetone solution and placed until the acetone on the surface evaporated. Then the bamboo strips were placed in anhydrous ethanol for ultrasonic cleaning for 10 minutes. Finally, the cleaned bamboo strips were taken out and placed in a vacuum drying oven at 45°C for drying. Then the bamboo strips were carbonized. The cleaned bamboo strips were evenly placed on high-temperature resistant alumina ceramic sheets and placed in a muffle furnace. Nitrogen was introduced to ensure that the carbonization was carried out in a nitrogen atmosphere. The carbonization was carried out at a temperature of 380°C for 40 minutes. Finally, the bamboo strips were taken out and placed in a sealed bag for later use.

[0073] Use a pipette to transfer 1000 μL of a 5 mg / mL silver nanowire solution to a 5 mL microcentrifuge tube, and then use a pipette to transfer 3000 μL of anhydrous ethanol to the same microcentrifuge tube, and then ultrasonicate for 30 minutes to prepare 4 mL of a 1.25 mg / mL silver nanowire solution.

[0074] 450 μL of 1.25 mg / mL silver nanowire ethanol solution was pipetted from a microcentrifuge tube and evenly applied on the dried carbonized bamboo substrate, and then placed in a vacuum drying oven for 4 hours. At this time, the sample was coated with one layer. Repeat this coating step twice, and three layers of 1.25 mg / mL silver nanowire solution were applied on the carbonized bamboo substrate.

[0075] Weigh 3.396g of AgNO3 and 17g of NaNO3 into a 500mL volumetric flask, then add deionized water to the scale line. After preparation, ultrasonicate for 20min to fully disperse AgNO3 and NaNO3 in the deionized water to prepare a mixed solution of 0.04mol / L AgNO3 and 0.4mol / L NaNO3. After preparation, ultrasonicate for 20min to fully disperse AgNO3 and NaNO3 in the deionized water.

[0076] The carbonized bamboo strips after drop coating with silver nanowires were used as working electrodes, the mixed solution of AgNO3 and NaNO3 was used as the deposition electrolyte solution, the mercurous sulfate electrode was used as the reference electrode, and the platinum electrode was used as the counter electrode. The potential was applied to -0.8V by constant potential deposition method, and the deposition time was set to 2000s to deposit nanosilver on the substrate surface. This deposition operation was repeated 4 times and placed in a vacuum drying oven to dry at 45°C.

[0077] Weigh 0.008 g of carboxylated multi-walled carbon nanotubes (CNT) into a 5 mL centrifuge tube, and then add 4 mL of anhydrous ethanol to prepare a 2 mg / mL carboxylated multi-walled carbon nanotube ethanol solution. After preparation, ultrasonicate for 40 minutes to fully disperse the carbon nanotubes in the ethanol to prepare a 2 mg / mL carboxylated multi-walled carbon nanotube ethanol solution.

[0078] Alternately and evenly drop dispersed carbon nanotube ethanol solution onto the carbonized bamboo substrate material on which nanosilver has been deposited, and use a pipette to transfer 450 μL of uniform and stable 2 mg / mL carboxylated multi-walled carbon nanotube ethanol solution and evenly drop it onto it. At this time, one layer of 2 mg / mL carboxylated multi-walled carbon nanotube ethanol solution has been drop-coated on the carbonized bamboo substrate material. Repeat this drop-coating step twice, that is, drop-coating three layers of carboxylated multi-walled carbon nanotube ethanol solution. A nanosilver composite carbon nanotube carbonized bamboo electrode can be obtained.

[0079] Example 4 Sensor Sample Preparation

[0080] The preparation process of sensor samples is as follows Figure 1 shown.

[0081] Cut the bamboo strips into 8cm×1cm×1cm specifications, then put the cut bamboo strips into deionized water for ultrasonic treatment for 10 minutes, then absorb the water on the surface of the bamboo strips and put them into acetone solution for ultrasonic treatment for 10 minutes, then take out the bamboo strips from the acetone solution and place them until the acetone on the surface evaporates, then put the bamboo strips into anhydrous ethanol for ultrasonic cleaning for 10 minutes, finally take out the cleaned bamboo strips and put them into a vacuum drying oven at 45°C for drying, then carbonize the bamboo strips, evenly place the cleaned bamboo strips on high-temperature resistant alumina ceramic sheets and put them into a muffle furnace, introduce nitrogen to ensure that the carbonization is in a nitrogen atmosphere, and carbonize at a temperature of 400°C for 40 minutes, finally take them out and put them in a sealed bag for use.

[0082] Use a pipette to transfer 2000 μL of a 5 mg / mL silver nanowire solution to a 5 mL microcentrifuge tube, then use a pipette to transfer 2000 μL of anhydrous ethanol to the same microcentrifuge tube, and then ultrasonicate for 30 minutes to prepare 4 mL of a 2.5 mg / mL silver nanowire solution.

[0083] 500 μL of 2.5 mg / mL silver nanowire ethanol solution was pipetted from a microcentrifuge tube and evenly dropped on the dried carbonized bamboo substrate, and then placed in a vacuum drying oven for 4 hours. At this time, the sample was drop-coated with one layer. Repeat this drop-coating step four times, and 5 layers of 2.5 mg / mL silver nanowire solution were drop-coated on the carbonized bamboo substrate.

[0084] Weigh 6.792g of AgNO3 and 34g of NaNO3 into a 500mL volumetric flask, then add deionized water to the scale line. After preparation, ultrasonicate for 20min to fully disperse AgNO3 and NaNO3 in the deionized water to prepare a mixed solution of 0.08mol / L AgNO3 and 0.8mol / L NaNO3. After preparation, ultrasonicate for 20min to fully disperse AgNO3 and NaNO3 in the deionized water.

[0085] The carbonized bamboo strips after drop coating with silver nanowires were used as working electrodes, the mixed solution of AgNO3 and NaNO3 was used as the deposition electrolyte solution, the mercurous sulfate electrode was used as the reference electrode, and the platinum electrode was used as the counter electrode. The potential was applied to -0.4V by constant potential deposition method, and the deposition time was set to 3000s to deposit nanosilver on the substrate surface. This deposition operation was repeated 4 times and placed in a vacuum drying oven to dry at 45°C.

[0086] Weigh 0.02 g of carboxylated multi-walled carbon nanotubes (CNT) into a 5 mL centrifuge tube, and then add 4 mL of anhydrous ethanol to prepare a 5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution. After preparation, ultrasonicate for 40 minutes to fully disperse the carbon nanotubes in the ethanol to prepare a 5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution.

[0087] Alternately and evenly drop dispersed carbon nanotube ethanol solution onto the carbonized bamboo substrate material on which nanosilver has been deposited, and use a pipette to transfer 500 μL of uniform and stable 5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution and evenly drop it onto it. At this time, one layer of 5 mg / mL carboxylated multi-walled carbon nanotube ethanol solution has been drop-coated onto the carbonized bamboo substrate material. Repeat this drop-coating step four times, i.e., five layers of carboxylated multi-walled carbon nanotube ethanol solution have been drop-coated. A nanosilver composite carbon nanotube carbonized bamboo electrode can be obtained.

[0088] Example 5 Reaction kinetics experiment of bio-based electrochemical sensor

[0089] The reaction kinetics experiment of bio-based electrochemical sensor was carried out on an electrochemical workstation with a concentration of 1 mmol / L -1 Potassium ferrocyanide-potassium ferrocyanide solution and 0.2 mol / L -1 The potassium chloride solution was used as the electrolyte and the measurement was carried out in a three-electrode system, wherein the reference electrode was a silver / silver chloride electrode, the counter electrode was a platinum sheet electrode, and the working electrode was a bio-based electrochemical sensor prepared according to Example 1 of the present invention. The effect of different scan rates on the working electrode was studied by changing the scan rate using cyclic voltammetry (CV). For CV measurement, the scan potential was between -1.6 and 1.6 V, and the scan rates were 10 m Vs -1 、30m Vs -1 , 50m Vs -1 、70m Vs -1 、100m Vs -1 、120m Vs -1 The experimental results are shown in the attached Figure 5 a and Figure 5 As shown in b, Figure 5b shows that the good linearity also proves that the experimental results are consistent with the electrochemical principles, and also verifies that the diffusion on the working electrode surface controls the electron transfer process and that a reversible electrochemical reaction occurs on the working electrode surface. This shows that the response current on the electrode surface consists of two parts, one is the Faraday current, that is, the current for the electrochemical reaction, and the other is the non-Faraday current, that is, the double-layer charging current. As the scan rate increases, the double-layer charging current increases, causing the current response on the electrode surface to increase, thereby increasing the redox peak current. The results show that a reversible electrochemical reaction occurs on the working electrode surface, and the electrode reaction kinetics is controlled by the diffusion process.

[0090] Example 6 Electrochemical impedance spectroscopy (EIS) experiment of bio-based electrochemical sensor

[0091] The electrochemical impedance test of the bio-based electrochemical sensor was carried out on an electrochemical workstation. A three-electrode system was used, in which the reference electrode was a silver / silver chloride electrode, the counter electrode was a platinum sheet electrode, and the working electrode was the bio-based electrochemical sensor prepared according to Example 1 of the present invention. -1 Potassium ferrocyanide-potassium ferrocyanide solution and 0.2 mol / L -1 The potassium chloride solution was used as the electrolyte and the measurement was carried out in a three-electrode system. The EIS analysis was carried out in the frequency range of 0.1~1000000 Hz and the signal amplitude was 0.01V. The experimental results are shown in the attached Figure 6 As shown in the figure, the impedance is located in the arc of the high frequency region and the straight line of the low frequency region, where the arc represents the electrochemical polarization process and the straight line represents the concentration polarization process. The semicircle diameter at the higher frequency represents the interface electron transfer resistance, which is equivalent to the charge transfer resistance, that is, the reaction resistance. The linear part at the low frequency corresponds to the diffusion process. The results show that the electrochemical sensor has a smaller charge transfer resistance (30.69ohm), indicating that the electrode surface has a stronger electron transfer ability and the electrode surface is more conducive to the occurrence of redox reactions.

[0092] Example 7 Electrochemical response experiment of formaldehyde

[0093] The electrochemical response experiment of formaldehyde was carried out on an electrochemical workstation using cyclic voltammetry (CV) and a traditional standard three-electrode system. The reference electrode was a silver / silver chloride electrode, the counter electrode was a platinum electrode, and the working electrode was a bio-based electrochemical sensor prepared according to Example 1 of the present invention. Formaldehyde NaOH solutions of different concentrations were prepared as electrolyte solutions using a 0.2 mol / L NaOH solution as a solvent, and then cyclic voltammetry was used with a scan range of -0.6 V to 0.6 V and a scan rate of 120 mV / s. The experimental results are shown in the attached figure. Figure 7 a and Figure 7 As shown in b, Figure 7a It can be seen that compared with the pure NaOH base solution (i.e. 0mM), the cyclic voltammetry curve of 0.5mmol / L-9mmol / L shows an obvious reduction peak, which means it has a good response. Figure 7 b It can be seen that the peak current and formaldehyde concentration show a good linear relationship in the range of 0.5mM-1.5 mM and 1.5mM-9 mM. The two linear ranges in the figure may be the result of the adsorption of the intermediate CO produced by the oxidation of HCHO onto the electrode. The mechanistic pathway of formaldehyde oxidation involves two possible pathways: a direct pathway (dehydrogenation) and an indirect pathway (dehydration) through the adsorption of CO as a poisoning substance. The indirect pathway involves the generation of CO, which is further oxidized to CO2. The formation of carbon dioxide will hinder the active surface sites. Therefore, the initial adsorption of the intermediate CO will reduce the sensitivity of the response, thereby producing a second linear range. The sensor prepared by the present invention has a good response to liquids and is particularly suitable for the detection of formaldehyde.

[0094] The above-described embodiments are only preferred embodiments of the present invention, but not all feasible embodiments of the present invention. For those skilled in the art, any obvious changes made thereto without departing from the principles and spirit of the present invention should be considered to be included in the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a multi-layer nano-network interlaced composite bio-based electrochemical sensor, characterized in that: The steps include: (1) Preparation of sensor substrate material: The cut bamboo pieces are ultrasonically cleaned and dried, and then carbonized. Finally, after cooling, the carbonized bamboo pieces are taken out for use to obtain the carbonized bamboo substrate material; (2) Preparation of silver nanowire ethanol solution: preparing a uniform silver nanowire ethanol solution; (3) Drip coating: evenly drip the dispersed silver nanowire ethanol solution onto the carbonized bamboo substrate; (4) Preparation of AgNO3 and NaNO3 mixed solution: prepare a uniform AgNO3 and NaNO3 mixed solution; (5) Electrochemical deposition: The carbonized bamboo strips coated with silver nanowires were used as working electrodes, a mixed solution of AgNO3 and NaNO3 was used as the deposition electrolyte solution, a mercurous sulfate electrode was used as the reference electrode, and a platinum electrode was used as the counter electrode. The nanosilver was deposited on the substrate surface by a constant potential deposition method, thus obtaining a nanosilver carbonized bamboo strip electrode. The deposition operation was repeated, and finally the electrode was dried. (6) Preparation of carbon nanotube ethanol solution: preparing a uniform carbon nanotube ethanol solution; (7) Construction of bio-based electrochemical sensor: The dispersed carbon nanotube ethanol solution is evenly dropped onto the nanosilver carbonized bamboo electrode to obtain the nanosilver composite carbon nanotube carbonized bamboo electrode; the bio-based electrochemical sensor with enhanced nanosilver network structure is constructed by electrochemical deposition method.

2. The method for preparing an electrochemical sensor according to claim 1, characterized in that: The bamboo pieces of step (1) have a specification range of 1-10 cm in length, 0.1-10 cm in width, and 0.01-4 cm in thickness; a carbonization temperature range of 300° C.-450° C.; and a carbonization time range of 20-60 min.

3. The method for preparing an electrochemical sensor according to claim 1, characterized in that: The concentration range of the silver nanowire ethanol solution in step (2) is 0.1 mg / mL-5 mg / mL.

4. The method for preparing an electrochemical sensor according to claim 1, wherein: The drip coating step in step (3) can be repeated for multiple layers, with a total number of drip coating layers of 1-14; the total amount of solution dripped in each layer ranges from 350 to 500 μL.

5. The method for preparing an electrochemical sensor according to claim 1, characterized in that: Step (4) The AgNO3 and NaNO3 mixed solution is composed of 0.01-0.1 mol / L AgNO3 and 0.1-1.0 mol / L NaNO3.

6. The method for preparing an electrochemical sensor according to claim 1, characterized in that: The constant potential deposition method in step (5) has a potential range of -1-0 V; a deposition time range of 800-3000 s; and a number of repeated deposition times of 1-6 times.

7. The method for preparing an electrochemical sensor according to claim 1, characterized in that: The concentration range of the carbon nanotube ethanol solution in step (6) is 0.1 mg / mL-5 mg / mL.

8. The method for preparing an electrochemical sensor according to claim 1, characterized in that: The drip coating step in step (7) can be repeated to coat multiple layers, with a total number of coating layers of 1-14; the total amount of carbon nanotube ethanol solution dripped in each layer ranges from 350 to 500 μL.

9. Application of the electrochemical sensor prepared by the method of claim 1, characterized in that: For liquid testing.