A γ-Al 2 O 3 / CF catalyst and preparation method thereof and method for synthesizing methyl chloride from methanol and hydrogen chloride
Through the microwave annealing and fluorination treatment of the γ-Al2O3/C-F catalyst, the problems of easy carbonization of the catalyst and high hydrogen chloride feed ratio are solved, efficient methanol and hydrogen chloride reaction is achieved, and resource waste and by-product generation are reduced.
Patent Information
- Application Number
- CN202411150848.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-21
AI Technical Summary
In the existing technology, when methanol reacts with hydrogen chloride, the catalyst γ-Al2O3 is easily carbonized, resulting in a decrease in efficiency, and the hydrogen chloride feed ratio is high, resulting in waste of resources and difficulty in controlling the content of the by-product dimethyl ether.
γ-Al2O3/C-F catalyst is used, carbon deposits are removed through microwave annealing treatment, and C-F bonds are formed by doping with fluorinating agent to improve the catalyst activity and reduce the hydrogen chloride feed ratio.
The catalyst is reused, the hydrogen chloride feed ratio is reduced, the methanol conversion rate and selectivity are maintained high, the generation of by-products is reduced, and resources and processing costs are saved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of methane chloride production, and particularly relates to a gamma-Al2O3 / CF catalyst and a preparation method thereof, and a method for synthesizing methyl chloride from methanol and hydrogen chloride. Background Art
[0002] Methyl chloride, also known as chloromethane or methyl chloride, is an organic compound with the chemical formula CH3Cl. Its main uses in industrial production are: (1) Methylating agent: Methyl chloride is an important source of methyl groups and is used in methylation reactions, such as the synthesis of methylchlorosilane (used to prepare silicone rubber, silicone resin, etc.), methyl mercaptan, etc.; (2) Synthesis of halogenated hydrocarbons: Methyl chloride can be used as an intermediate in the preparation of halogenated hydrocarbons such as dichloromethane, trichloromethane, and carbon tetrachloride; (3) Refrigerants and foaming agents: Methyl chloride is used as an important component in the production of refrigeration equipment, refrigerants and foaming agents; (4) Organic solvent: Methyl chloride can be used as an organic solvent and is widely used in the fields of chemical industry, pharmaceuticals, pesticides, etc.; (5) Local anesthetic: Methyl chloride was once used as a local anesthetic, although its use in the medical field has gradually decreased.
[0003] At present, the method for producing chloromethane in China is mainly to react gaseous methanol with hydrogen chloride in a fixed bed reactor equipped with γ-Al2O3 catalyst. There are two problems with this method. First, in 220 o C~260 o At reaction temperatures of 100°C, the raw methanol easily carbonizes, covering the active sites of the catalyst's γ-Al₂O₃ and clogging its pores, ultimately leading to decreased catalyst efficiency or even deactivation. Furthermore, during the reaction, some of the γ-Al₂O₃ undergoes a phase transformation to form inactive boehmite (AlO(OH)), which can also cause catalyst deactivation. Due to the low usage and long lifespan of the catalyst, deactivated catalysts are typically disposed of directly as solid waste. This treatment method not only increases production costs and the risk of secondary pollution, but also wastes resources. Secondly, to reduce the byproduct dimethyl ether content and maintain a high conversion rate in this reaction, the molar ratio of methanol to hydrogen chloride must be controlled within a range of 1:1.15 to 1.2 during the feed. However, after the reaction, the excess hydrogen chloride and the product monochloromethane must be separated by washing with water or acid, resulting in significant consumption of the raw hydrogen chloride and the water or acid wash solution. Therefore, reducing the feed ratio of hydrogen chloride in the production of monochloromethane has become an urgent technical challenge.
[0004] Patent document CN116196965A discloses a γ-Al2O3 / CN catalyst and its preparation method. The γ-Al2O3 / CN catalyst is derived from deactivated γ-Al2O3 catalyst produced during the hydrochlorination of methanol to methyl chloride. The γ-Al2O3 / CN catalyst contains C-N and C=N bonds, and nitrogen-doped carbon is uniformly distributed on the surface of the γ-Al2O3. The γ-Al2O3 / CN catalyst prepared by this method not only fully utilizes the deactivated γ-Al2O3 / CN catalyst, which is typically treated as hazardous waste, but also exhibits higher catalytic activity than fresh γ-Al2O3 catalyst. However, the inventors' research has found that while the γ-Al2O3 / CN catalyst prepared in this patent document maintains high catalytic efficiency at a methanol:hydrogen chloride molar ratio of 1:1.15, like fresh γ-Al2O3 catalyst, its catalytic efficiency decreases with decreasing hydrogen chloride feed ratio. That is, the γ-Al2O3 / CN catalyst prepared by this method still cannot achieve the purpose of reducing the feed ratio of hydrogen chloride. Summary of the Invention
[0005] The present invention provides a γ-Al2O3 / CF catalyst that can reuse deactivated γ-Al2O3 produced in the production of methanol-hydrochloride-methylene chloride. Furthermore, the catalyst can also reduce the feed ratio of hydrogen chloride in the production of methanol-hydrochloride-methylene chloride. Specifically, the following scheme is adopted:
[0006] A γ-Al2O3 / CF catalyst, characterized in that fluorine-doped carbon is uniformly distributed on the surface of γ-Al2O3, the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst is 58-76%, and the proportion of CF covalent bonds formed by fluorine doping is 24-42%.
[0007] Preferably, in the γ-Al2O3 / CF catalyst, the proportion of CF semi-ionic bonds formed by fluorine doping is 71-76%, and the proportion of CF covalent bonds formed by fluorine doping is 24-29%.
[0008] Furthermore, the specific surface area of the γ-Al2O3 / CF catalyst is 182-186 sqm, and the most probable pore diameter is 9.2-9.56 nm.
[0009] Typically, the fresh γ-Al2O3 catalyst used in the vapor-phase production of methyl chloride under existing process conditions is a white Raschig ring with an outer diameter of 3.95-4.05 mm, an inner diameter of 1-2 mm, a height of 3.9-4.1 mm, a specific surface area of 190-191 sqm, and a most probable pore size of 9.6-9.8 nm. From a macroscopic perspective, the deactivated catalyst only changes color from white to black, while retaining the Raschig ring appearance. The deactivated γ-Al2O3 catalyst has a specific surface area of 178-179 sqm and a most probable pore size of 8.5-8.7 nm.
[0010] In the prior art, to restore deactivated catalysts to meet the needs of daily production, high-temperature calcination is typically used to regenerate catalysts deactivated by carbon deposition. However, after experimenting with traditional high-temperature calcination methods for deactivated γ-Al2O3 catalysts produced during the vapor-phase preparation of methyl chloride, the inventors discovered that this only partially restored the activity of the γ-Al2O3 catalyst, far from achieving the conversion rate and service life required for normal production.
[0011] Based on this, the present invention also discloses a method for preparing the above-mentioned γ-Al2O3 / CF catalyst, comprising the following steps:
[0012] (1) Preparation of γ-Al2O3 / C 1-X : The deactivated γ-Al2O3 produced in the production of methanol-hydrogen chloride to methyl chloride was placed in a microwave muffle furnace and annealed in air atmosphere to obtain γ-Al2O3 / C 1-X , where X represents the amount of carbon deposits removed by annealing, and 1-X represents the amount of carbon deposits remaining after annealing;
[0013] (2) Preparation of γ-Al2O3 / CF: The γ-Al2O3 / C obtained in step (1) 1-X Fluorine element was doped with a fluorinating agent under a nitrogen atmosphere to obtain a γ-Al2O3 / CF catalyst.
[0014] The preparation method of the present invention uses γ-Al2O3 deactivated during the production of methyl chloride by a gas phase process as a raw material. First, the deactivated catalyst is placed in a microwave muffle furnace and annealed in an air atmosphere. Compared with traditional thermal radiation heating, microwave heating can heat the object more quickly and evenly. It is easier to evenly remove carbon deposits formed by methanol inside and outside the catalyst pores by adjusting the holding time during the annealing treatment, providing the possibility of subsequently restoring the catalyst pore structure and forming more evenly distributed fluorination sites. At the same time, by controlling the holding temperature during annealing, the inactive boehmite AlO(OH) in the deactivated catalyst γ-Al2O3 can be converted back into active γ-Al2O3.
[0015] Then, fluorine doping was performed by a fluorinating agent to convert the γ-Al2O3 / C 1-X The γ-Al2O3 / CF catalyst was transformed into a fluorine-doped carbon, which produced more new active sites, enhanced the electron transfer efficiency in the γ-Al2O3 catalytic process, constructed a synergistic catalytic effect between metal and non-metal structures, and further improved the catalyst activity. The γ-Al2O3 / CF catalyst prepared by the above method has better performance than the newly purchased catalyst.
[0016] Furthermore, the temperature of fluorine doping in step (2) is 100~250 o C, the fluorine doping time is 10~50 min, the mass fraction ratio of fluorinating agent / nitrogen is 0.02~0.1:1, and the feed rate of the mixed gas of fluorinating agent and nitrogen is 50~300 ml / min.
[0017] The inventors found that the reaction temperature, reaction time, mass fraction ratio of fluorinating agent / nitrogen and the feed amount of the mixed gas of fluorinating agent and nitrogen in the fluorination process directly affect the ratio of CF covalent bonds and semi-ionic bonds in the prepared γ-Al2O3 / CF catalyst. o C, a fluorine doping time of 10-50 minutes, a fluorinating agent / nitrogen mass ratio of 0.02-0.1:1, and a fluorinating agent / nitrogen mixed gas feed rate of 50-300 ml / min favor the transformation of C-F bonds from covalent bonds to semi-ionic bonds. The inventors also discovered that in the γ-Al2O3 / CF3 catalyst-catalyzed synthesis of methyl chloride from methanol and hydrogen chloride, a greater proportion of C-F semi-ionic bonds in the catalyst significantly improves catalytic efficiency.
[0018] Preferably, the temperature of fluorine doping in step (2) is 180~220 o C, the fluorine doping time is 15~40 min, the mass fraction ratio of fluorinating agent / nitrogen is 0.03~0.06:1, and the feed rate of the mixed gas of fluorinating agent and nitrogen is 180~220 ml / min.
[0019] Furthermore, the annealing temperature in step (1) is 450~750 o C, the microwave output power of the annealing treatment is 400~1000W, and the holding time of the annealing treatment is 0.5-2h.
[0020] Preferably, the microwave output power during the annealing treatment in step (1) is 650W, and the annealing temperature is 650 o C, the holding time of annealing treatment is 1h.
[0021] The microwave output power during the annealing treatment directly affects the distribution and pore structure of the amorphous carbon. Excessive microwave power will lead to uneven amorphous carbon distribution and easily further damage the pore structure, causing irreparable damage. However, too low a microwave power will result in excessively long treatment times, which is not conducive to mass production. Therefore, the preferred microwave power during the annealing treatment is 650W.
[0022] Annealing temperature directly affects the content of amorphous carbon. When the holding time is 1h and the annealing temperature is 350 o C, after the treated catalyst was cut open, the outer surface and the cut surface were still black, indicating that the carbon deposits were difficult to remove at this temperature. o C, the outer surface of the annealed catalyst turned yellow-brown, the inner surface turned light gray, and the carbon deposits were removed. o C, compared with the fresh catalyst, the surface and cross section of the treated catalyst still have a little yellow. o C, still can not completely restore the pure white, and the catalyst powder is serious, which means that simple annealing treatment cannot completely remove the carbon deposits. Therefore, the annealing temperature should be controlled at 450~750 o C, the preferred annealing temperature is 650 o C.
[0023] Furthermore, the fluorinating agent is any one of fluorine gas, xenon difluoride, xenon tetrafluoride and sulfur tetrafluoride.
[0024] The present invention also discloses a method for synthesizing methyl chloride from methanol and hydrogen chloride, which is catalyzed by using any of the above-mentioned γ-Al2O3 / CF catalysts or the γ-Al2O3 / CF catalysts prepared by any of the above-mentioned preparation methods.
[0025] Furthermore, in the above-mentioned method for synthesizing methyl chloride from methanol and hydrogen chloride, the feed molar ratio of methanol to hydrogen chloride is 1:1.1, the methanol conversion is ≥99.6%, and the methyl chloride selectivity is ≥99.8%. Due to the use of the γ-Al2O3 / CF catalyst of the present invention, the feed ratio of hydrogen chloride can be reduced while maintaining a high methanol conversion and methanol selectivity.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The γ-Al2O3 / CF catalyst of the present invention not only reuses the deactivated γ-Al2O3 catalyst, saving the cost of purchasing fresh catalyst and disposing of waste catalyst, but also, in the methyl chloride synthesis reaction using the γ-Al2O3 / CF catalyst of the present invention, after reducing the proportion of hydrogen chloride, the methanol selectivity and conversion rate of the reaction can still be maintained at a high level, which greatly facilitates the separation of the product methyl chloride and hydrogen chloride, effectively controls the output of the by-product hydrochloric acid, and brings multiple benefits to the company. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below.
[0029] Unless otherwise specified, the reagents, equipment and materials described in the following examples and experimental examples are all prior art and can be obtained from commercial channels.
[0030] Among them, 1. The thermogravimetric analyzer model used for thermogravimetric analysis is NETZSCH STA409C.
[0031] 2. The X-ray diffractometer used for XRD measurement is the Dmax-Ultima model of Japan Rigaku Corporation.
[0032] 3. The gas chromatograph used for gas chromatography analysis was Shimadzu 2010-PRO.
[0033] Example 1
[0034] This embodiment discloses a method for preparing a γ-Al2O3 / CF catalyst:
[0035] (1) Preparation of γ-Al2O3 / C 1-X The γ-Al2O3 catalyst deactivated in the production of chloromethane by methanol vapor phase process was placed in a microwave muffle furnace and annealed in air atmosphere at a temperature of 650 o C, microwave power was controlled at 650W, and the holding time was 1h; the obtained γ-Al2O3 / C was obtained by thermogravimetric analysis. 1-X The carbon content is 0.9wt%.
[0036] (2) Preparation of γ-Al2O3 / CF: Take 100 g of γ-Al2O3 / C 1-X Spread them evenly in two layers on a grid with small holes. Turn on the heating before the reaction starts. Continue to introduce high-purity nitrogen into the reactor at a rate of 100 ml / min. Continue to ventilate for 1 hour after reaching the reaction temperature to ensure that there is no water vapor in the reactor to prevent corrosion of equipment and affect the fluorination effect. When the fluorine / nitrogen mass fraction ratio is 0.05:1, the feed rate of fluorine and nitrogen mixture is 200 ml / min, and the fluorination temperature is 200 oC, fluorine doping was performed under the condition of fluorination time of 30 min to obtain γ-Al2O3 / CF catalyst.
[0037] The fresh white Raschig ring γ-Al2O3 catalyst used in the production of chloromethane by the methanol vapor phase process has an outer diameter of 4.0 mm, an inner diameter of 1.4 mm, a height of 3.95 mm, a specific surface area of 190.5 sqm, and a most probable diameter of 9.7 nm.
[0038] The specific surface area of the deactivated blackened Raschig ring γ-Al2O3 catalyst was reduced to 184 sqm, and the most probable pore diameter was 9.2 nm.
[0039] There are many tiny pore structures inside the fresh γ-Al2O3 catalyst.
[0040] The surface of the deactivated γ-Al2O3 catalyst is covered with a layer of mesh-like carbon deposits; this reduces the specific surface area and the most probable pore size of the deactivated catalyst to 184 sqm and 9.2 nm.
[0041] In addition, the phase structure of the deactivated catalyst also changes, generating inactive AlO(OH).
[0042] By controlling the microwave power, holding time and holding time, the γ-Al2O3 / C 1-X The carbon in the catalyst is evenly distributed on the surface of the catalyst, laying the foundation for the next step of fluorination.
[0043] After 650 o After C annealing treatment, AlO(OH) has been completely transformed into γ-Al2O3.
[0044] XPS analysis shows that in the γ-Al2O3 / CF catalyst prepared in this embodiment, the proportion of CF semi-ionic bonds formed by fluorine doping is 75.56%, and the proportion of CF covalent bonds formed by fluorine doping is 24.44%.
[0045] Example 2
[0046] The only difference between this embodiment and embodiment 1 is that: Step (1) prepares γ-Al2O3 / C 1-X The annealing temperature was controlled at 550 o C, microwave power was controlled at 400W, and the holding time was 0.5h. The obtained γ-Al2O3 / C was obtained by thermogravimetric analysis. 1-X The carbon content is 1.2wt%.
[0047] Other preparation conditions are exactly the same as those in Example 1.
[0048] Example 3
[0049] The only difference between this embodiment and embodiment 1 is that: Step (1) prepares γ-Al2O3 / C 1-X The annealing temperature was controlled at 750 o C, microwave power was controlled at 1000W, and the heat preservation time was 2h. The obtained γ-Al2O3 / C was obtained by thermogravimetric analysis. 1-X The carbon content is 0.4wt%.
[0050] Other preparation conditions are exactly the same as those in Example 1.
[0051] Example 4
[0052] The only difference between this embodiment and embodiment 1 is that in step (2) when preparing γ-Al2O3 / CF, the mass fraction ratio of fluorine gas to nitrogen gas is 0.02:1, the feed rate of fluorine gas and nitrogen mixed gas is 50ml / min, and the fluorination temperature is 100 o C, fluorination time is 10 min.
[0053] Other preparation conditions are exactly the same as those in Example 1.
[0054] XPS verification showed that in the γ-Al2O3 / CF catalyst prepared in this embodiment, the proportion of CF semi-ionic bonds formed by fluorine doping was 59.48%, and the proportion of CF covalent bonds formed by fluorine doping was 40.52%.
[0055] Example 5
[0056] The only difference between this embodiment and embodiment 1 is that in step (2) when preparing γ-Al2O3 / CF, the fluorine gas / nitrogen gas mass fraction ratio is 0.1:1, the feed rate of the fluorine gas and nitrogen mixed gas is 300 ml / min, and the fluorination temperature is 250 o C, fluorination time is 50 min.
[0057] Other preparation conditions are exactly the same as those in Example 1.
[0058] XPS analysis showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this embodiment was 67.39%, and the proportion of CF covalent bonds formed by fluorine doping was 32.61%.
[0059] Comparative Example 1
[0060] The only difference between this comparative example and Example 1 is that the step (2) of preparing γ-Al2O3 / CF is omitted. The other preparation conditions are exactly the same as those in Example 1.
[0061] Comparative Example 2
[0062] The difference between this comparative example and Example 1 is that: Step (1) prepares γ-Al2O3 / C1-X The annealing temperature was controlled at 350 o C. Through thermogravimetric analysis, the obtained γ-Al2O3 / C 1-X The carbon content is 1.6wt%.
[0063] Other preparation conditions are exactly the same as those in Example 1.
[0064] Comparative Example 3
[0065] The difference between this comparative example and Example 1 is that: Step (1) prepares γ-Al2O3 / C 1-X The annealing temperature was controlled at 850 o C. Through thermogravimetric analysis, the obtained γ-Al2O3 / C 1-X The carbon content is 0.2wt%.
[0066] Other preparation conditions are exactly the same as those in Example 1.
[0067] Comparative Example 4
[0068] This comparative example discloses a method for preparing a γ-Al2O3 / CN catalyst, which is prepared by adopting the most preferred solution disclosed in the patent document with publication number CN116196965A, that is, the preparation method disclosed in Example 1 in CN116196965A.
[0069] Comparative Example 5
[0070] The only difference between this comparative example and Example 1 is that in step (2) when preparing γ-Al2O3 / CF, the fluorination temperature is 50 o C, and other preparation conditions are exactly the same as those in Example 1.
[0071] XPS verification showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this comparative example was 29.77%, and the proportion of CF covalent bonds formed by fluorine doping was 70.23%.
[0072] Comparative Example 6
[0073] The only difference between this comparative example and Example 1 is that in step (2) when preparing γ-Al2O3 / CF, the fluorination temperature is 350 o C, and other preparation conditions are exactly the same as those in Example 1.
[0074] XPS verification showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this comparative example was 40.56%, and the proportion of CF covalent bonds formed by fluorine doping was 59.44%.
[0075] Comparative Example 7
[0076] The only difference between this comparative example and Example 1 is that in step (2) when preparing γ-Al2O3 / CF, the fluorination time is 2 minutes, and the other preparation conditions are exactly the same as those in Example 1.
[0077] XPS verification showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this comparative example was 35.44%, and the proportion of CF covalent bonds formed by fluorine doping was 64.56%.
[0078] Comparative Example 8
[0079] The only difference between this comparative example and Example 1 is that in step (2) when preparing γ-Al2O3 / CF, the fluorination time is 70 min, and the other preparation conditions are exactly the same as those in Example 1.
[0080] XPS verification showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this comparative example was 29.23%, and the proportion of CF covalent bonds formed by fluorine doping was 70.77%.
[0081] Comparative Example 9
[0082] The only difference between this comparative example and Example 1 is that in step (2) when preparing γ-Al2O3 / CF, the mass fraction ratio of fluorine gas to nitrogen gas is 0.005:1, and the other preparation conditions are exactly the same as those in Example 1.
[0083] XPS verification showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this comparative example was 48.84%, and the proportion of CF covalent bonds formed by fluorine doping was 51.16%.
[0084] Comparative Example 10
[0085] The only difference between this comparative example and Example 1 is that in step (2) when preparing γ-Al2O3 / CF, the mass fraction ratio of fluorine gas to nitrogen gas is 0.2:1, and the other preparation conditions are exactly the same as those in Example 1.
[0086] XPS verification showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this comparative example was 30.78%, and the proportion of CF covalent bonds formed by fluorine doping was 69.22%.
[0087] Comparative Example 11
[0088] The only difference between this comparative example and Example 1 is that in step (2) when preparing γ-Al2O3 / CF, the feed rate of the mixed gas of fluorine and nitrogen is 25 ml / min, and the other preparation conditions are exactly the same as those in Example 1.
[0089] XPS verification showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this comparative example was 38.37%, and the proportion of CF covalent bonds formed by fluorine doping was 61.63%.
[0090] Comparative Example 12
[0091] The only difference between this comparative example and Example 1 is that in step (2) when preparing γ-Al2O3 / CF, the feed rate of the mixed gas of fluorine and nitrogen is 350 ml / min, and the other preparation conditions are exactly the same as those in Example 1.
[0092] XPS verification showed that the proportion of CF semi-ionic bonds formed by fluorine doping in the γ-Al2O3 / CF catalyst prepared in this comparative example was 42.66%, and the proportion of CF covalent bonds formed by fluorine doping was 57.34%.
[0093] Experimental Example 1
[0094] 1. Experimental Purpose: To evaluate the catalytic efficiency of the catalysts prepared in Examples 1-5, fresh γ-Al2O3 catalysts, and the catalysts prepared in Comparative Examples 1-8.
[0095] II. Experimental Method: Each of the catalysts obtained above was used to catalyze the production of methyl chloride by a methanol vapor phase process. Specific conditions were: a methanol to hydrogen chloride molar ratio of 1:1 to 1.15 (the molar ratio of methanol to hydrogen chloride in conventional production is 1:1.15), a reaction temperature of 240°C, and a pressure of 0.2 MPa. The mixed gases produced using the different catalysts were analyzed by gas chromatography to determine conversion and selectivity.
[0096] 3. Experimental Results
[0097] When the molar ratio of methanol to hydrogen chloride is 1:1.15, the specific results are shown in Table 1:
[0098] Table 1 Catalytic efficiency indexes of various catalysts
[0099]
[0100] Except for changing the feed molar ratio of methanol and hydrogen chloride, the other reaction conditions remained unchanged, and the catalytic efficiency indicators of the fresh γ-Al2O3 catalyst, the catalyst prepared in Example 1, and the catalyst prepared in Comparative Example 4 were tested. The specific results are shown in Tables 2 and 3.
[0101] Table 2 Catalytic efficiency indexes of fresh catalyst and catalyst prepared in Example 1
[0102]
[0103] Table 3 Catalytic efficiency indexes of the catalyst prepared in Comparative Example 4 and the catalyst prepared in Example 1
[0104]
[0105] From the data analysis in Table 1, it can be seen that the initial methanol conversion rate of the fresh γ-Al2O3 catalyst is 99.56%, and the initial chloroform selectivity is 99.61%; after 360 hours, the methanol conversion rate is 99.49%, and after 360 hours, the chloroform selectivity is 99.52%.
[0106] The γ-Al2O3 / CF catalyst obtained in Example 1 achieved an initial methanol conversion rate and methyl chloride selectivity of 99.82% and 99.91%, respectively, exceeding even the efficiency of fresh γ-Al2O3 catalyst. After 360 hours, the methanol conversion rate was 99.78%, and the methyl chloride selectivity was 99.88%, demonstrating good cyclic stability. Examples 2 through 5 also exhibited excellent cyclic stability.
[0107] The catalytic efficiency of the catalysts prepared in Comparative Examples 1 to 3 decreased significantly after 360 hours, and their cyclic stability was poor.
[0108] The initial methanol conversion rate and methyl chloride selectivity of the γ-Al2O3 / CN catalyst prepared in Comparative Example 4 were slightly higher than those of the fresh catalyst, but were still slightly insufficient compared to those in Example 1.
[0109] The methanol conversion rate and selectivity of the catalysts prepared in Comparative Examples 5 to 12 were both lower than 95%. Compared with the results of the examples, it can be concluded that when the fluorination temperature is controlled at 100 to 250 o When the fluorination time is controlled within the range of 10-50 min, the mass fraction ratio of the fluorinating agent to nitrogen is controlled within the range of 0.03-0.06:1, and the feed rate of the mixed gas of the fluorinating agent and nitrogen is controlled within the range of 180-220 ml / min, the proportion of CF semi-ionic bonds formed by fluorine doping in the prepared γ-Al2O3 / CF catalyst can be controlled to be higher than that of CF covalent bonds, and when the proportion of CF semi-ionic bonds is higher, the catalytic performance of the catalyst is better.
[0110] Analysis of the data in Table 2 shows that the catalytic efficiency of the fresh γ-Al2O3 catalyst decreases continuously with decreasing HCl feed ratios, significantly shortening the catalyst lifespan. However, the catalytic efficiency of the γ-Al2O3 / CF catalyst prepared in Example 1 did not decrease when the methanol to HCl ratio dropped to 1:1.1, but began to decline when the methanol to HCl ratio dropped to 1:1.05. This demonstrates that the catalyst in Example 1 can maintain a high catalytic performance even at a 1:1.1 methanol to HCl feed ratio, successfully reducing the HCl ratio from 1:1.15 to 1:1.10.
[0111] Analysis of the data in Table 3 shows that while the catalyst prepared in Comparative Example 4 exhibits superior cycle stability, its initial methanol conversion and selectivity decrease significantly with decreasing hydrogen chloride content. However, the catalyst prepared in Example 1 still maintains an initial methanol selectivity of 99.90% and a methanol conversion of 99.82% at a methanol:hydrogen chloride molar ratio of 1:1.1. Therefore, in actual production, the use of the γ-Al2O3 / CF catalyst of the present invention can reduce the hydrogen chloride feed ratio, greatly facilitating the separation of the products monochloromethane and hydrogen chloride while also reducing the consumption of hydrogen chloride and the aqueous or pickling solution used during separation.
Claims
1. A γ-Al 2 O 3 / CF catalyst, It is characterized in that Deactivated γ-Al generated in the production of chloromethane by methanol-hydrochlorination gas phase method 2 O 3 The catalyst is raw material, and fluorine-doped carbon is evenly distributed in γ-Al 2 O 3 The surface of the γ-Al 2 O 3 In the / CF catalyst, the proportion of CF semi-ionic bonds formed by fluorine doping is 58~76%, and the proportion of CF covalent bonds formed by fluorine doping is 24~42%.
2. The γ-Al according to claim 1 2 O 3 / CF catalyst, It is characterized in that The γ-Al 2 O 3 In the / CF catalyst, the proportion of CF semi-ionic bonds formed by fluorine doping is 71~76%, and the proportion of CF covalent bonds formed by fluorine doping is 24~29%.
3. The γ-Al according to claim 1 2 O 3 / CF catalyst, It is characterized in that The γ-Al 2 O 3 The specific surface area of the CF / CF catalyst is 182-186 sqm, and the most probable pore size is 9.2-9.56 nm.
4. A γ-Al according to any one of claims 1 to 3 2 O 3 / Preparation method of CF catalyst, It is characterized in that The steps include: (1) Preparation of γ-Al 2 O 3 / C 1-X :The deactivated γ-Al produced in the production of methyl chloride by the methanol-hydrogen chloride gas phase method 2 O 3 The catalyst was placed in a microwave muffle furnace and annealed in air to obtain γ-Al 2 O 3 / C 1-X , where X represents the amount of carbon deposits removed by annealing, and 1-X represents the amount of carbon deposits remaining after annealing; (2) Preparation of γ-Al 2 O 3 / CF: The γ-Al obtained in step (1) 2 O 3 / C 1-X Fluorinization agent was used to dope fluorine in nitrogen atmosphere to obtain γ-Al 2 O 3 / CF catalyst.
5. The γ-Al according to claim 4 2 O 3 / Preparation method of CF catalyst, It is characterized in that In step (2), the fluorine doping temperature is 100-250° C., the fluorine doping time is 10-50 min, the mass fraction ratio of the fluorinating agent to the nitrogen is 0.02-0.1:1, and the feed rate of the mixed gas of the fluorinating agent and the nitrogen is 50-300 mL / min.
6. The method for preparing the γ-Al2O3 / CF catalyst according to claim 4, It is characterized in that In step (2), the fluorine doping temperature is 180-220° C., the fluorine doping time is 15-40 min, the mass fraction ratio of the fluorinating agent to the nitrogen is 0.03-0.06:1, and the feed rate of the mixed gas of the fluorinating agent and the nitrogen is 180-220 mL / min.
7. The γ-Al according to claim 4 2 O 3 / Preparation method of CF catalyst, It is characterized in that The temperature of the annealing treatment in step (1) is 450-750° C., the microwave output power of the annealing treatment is 400-1000 W, and the insulation time of the annealing treatment is 0.5-2 h.
8. The γ-Al according to claim 4 2 O 3 / Preparation method of CF catalyst, It is characterized in that The fluorinating agent is any one of fluorine gas, xenon difluoride, xenon tetrafluoride and sulfur tetrafluoride.
9. A method for synthesizing methyl chloride from methanol and hydrogen chloride, It is characterized in that Using the γ-Al described in any one of claims 1 to 3 2 O 3 / CF catalyst or γ-Al prepared by the preparation method according to any one of claims 4 to 8 2 O 3 / CF catalyst for catalysis.