A thermal shock and slag resistant magnesium carbon based composite refractory brick and its preparation method

Through the combination of artificially modified carbon and granulated modified titanium-containing blast furnace slag, the performance degradation of magnesium carbon bricks in high-temperature oxidative atmosphere is solved, the resistance to thermal shock and slag corrosion is improved, and the service life is extended. Improved overall performance.

CN118666570BActive Publication Date: 2024-11-12LIAONING ZHAOFENG CHANGSHENG SPECIAL REFRACTORY MATERIALS (GRP) CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411167493.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing magnesium carbon bricks are easily oxidized under high-temperature oxidative atmosphere, their thermal shock resistance and slag corrosion resistance are reduced, their service life is short, and the addition of graphite affects strength and oxidation resistance, and it is difficult to comprehensively improve their performance with each other.

Method used

Use artificially modified carbon and granulated modified titanium-containing blast furnace slag to combine, with good homogeneity and high hardness. The cladding and pore filling structure are formed through specific processes to improve the room temperature and compressive strength and high temperature folding resistance of refractory bricks. Strength, enhance thermal shock resistance and slag corrosion resistance.

Benefits of technology

The preparation of high-quality refractory bricks is achieved, extending service life, improving thermal shock resistance and slag corrosion resistance, reducing the risk of thermal stress cracks, and improving overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to a heat shock and slag resistant magnesium carbon-based composite refractory brick and a preparation method thereof, belonging to the technical field of refractory materials, wherein the refractory brick components include dead-burned magnesium oxide, artificial modified carbon, granulated modified titanium-containing blast furnace slag and phenolic resin; the artificial modified carbon is prepared by coating the surface of calcined petroleum coke powder with molybdenum disilicide powder and spinning asphalt powder, and then performing modification and sintering treatment. Granulated modified titanium-containing blast furnace slag is prepared by dry ball milling titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch, and then mixing with water and ZS-1071 high temperature resistant inorganic adhesive, briquetting, sintering and crushing. Artificial modified carbon and granulated modified titanium-containing blast furnace slag are used in combination, and each component material has good homogeneity and high hardness, and can realize high pressure pressing and high temperature heat treatment to obtain high-quality refractory bricks, which can effectively improve the room temperature compressive strength, high temperature flexural strength, thermal shock resistance and slag erosion resistance of refractory bricks, realize the comprehensive improvement of various indicators and extend the service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a heat-shock-resistant and slag-resistant magnesium-carbon-based composite refractory brick and a preparation method thereof. Background Art

[0002] Magnesia carbon brick is a commonly used refractory material. The main formula of magnesia carbon brick usually contains magnesia sand, graphite and binder. Among them, magnesia sand has good chemical stability, plays a role in high temperature resistance and corrosion resistance, graphite helps to improve thermal conductivity, thermal shock resistance and slag corrosion resistance, and the binder has the function of bonding and molding, which can closely combine various components.

[0003] Magnesia carbon bricks are widely used and play an important role in many high-temperature industrial fields. In the iron and steel metallurgical industry, they are indispensable lining materials or key components for steelmaking converters, electric furnaces, ladles, tundishes, etc. The temperature in the steelmaking process is extremely high and the melt is highly corrosive. Magnesia carbon bricks can withstand this harsh environment well and provide guarantees for the smooth progress of steelmaking. In other metal smelting, they are used in key parts or linings of smelting furnaces, refining furnaces, and insulation furnaces. They can adapt to frequent changes in temperature in the furnace, resist the erosion of the melt, and reduce the risk of damage to the lining. In addition, they can also be used in cement kilns and melting furnaces in the glass industry.

[0004] Although magnesia carbon bricks are a mature technology and basically meet the existing use requirements, there are still some technical bottlenecks, which lead to the short service life of refractory bricks and the need for regular replacement and maintenance. That is, under high temperature and oxidizing atmosphere, magnesia carbon bricks are easily oxidized, and the ability to resist thermal shock and slag erosion will decrease, shortening the service life. Although various antioxidants are added to improve the oxidation resistance, the strength and oxidation resistance will decrease due to the addition of graphite components. In addition, if the various reinforcing additives are not mixed properly or the quality is uneven, there will be a problem of significant performance degradation, such as poor crack resistance, wear resistance, and thermal shock resistance. Therefore, the use of various components has the problem of mutual checks and balances of performance, and it is difficult to achieve a comprehensive improvement in overall performance.

[0005] With the continuous development of technology in various industries, the high quality requirements for refractory bricks are getting higher and higher. Therefore, it is necessary to continuously improve and enhance the various properties of refractory bricks to meet the increasing requirements of use. Summary of the invention

[0006] The existing magnesium carbon bricks are easily oxidized during use, and the thermal shock resistance and the ability to resist slag erosion will decrease, shortening the service life; although adding graphite can improve the thermal shock resistance, it will affect the strength and oxidation resistance of magnesium carbon bricks. For example, the ladle uses magnesium carbon brick lining, and the graphite component has poor resistance to slag erosion and erosion. Graphite easily enters the furnace water, affecting the stability of the furnace water component; the use of various components of magnesium carbon bricks still has the problem of mutual balance of performance, and it is difficult to achieve comprehensive improvement of overall performance. The present invention provides a thermal shock and slag resistant magnesium carbon-based composite refractory brick and a preparation method thereof, which adopts artificial modified carbon and granulated modified titanium-containing blast furnace slag for use. The homogeneity of each component material is good, the hardness is high, and it can achieve compression molding at a pressure of 250MPa to 280MPa. It will not cause uneven thermal stress and thermal stress cracks at a high temperature of 270℃ to 290℃, and can achieve the preparation of high-quality refractory bricks. The combination of artificial modified carbon and granulated modified titanium-containing blast furnace slag can effectively improve the room temperature compressive strength and high temperature flexural strength of refractory bricks, and has outstanding thermal shock resistance and slag erosion resistance, which can greatly improve the thermal shock resistance and the ability to resist slag erosion, achieve comprehensive improvement of various indicators, and extend service life. The specific technical solution is as follows:

[0007] A heat-shock-resistant and slag-resistant magnesium-carbon-based composite refractory brick, the refractory brick comprising the following raw materials in parts by weight: 70 to 80 parts of dead-burned magnesium oxide, 10 to 15 parts of artificial modified carbon, 5 to 8 parts of granulated modified titanium-containing blast furnace slag, and 3 to 5 parts of phenolic resin;

[0008] The preparation method of artificial modified carbon is as follows: according to the mass ratio of calcined petroleum coke powder: molybdenum disilicide powder: spinning pitch powder = 100: (3-5): (1.5-2.5), calcined petroleum coke powder with a median particle size of 10 μm-25 μm, nano-scale molybdenum disilicide powder and nano-scale spinning pitch powder are evenly mixed by air flow to obtain mixed powder A; the mixed powder A is placed in a reactor, modified at 360°C-450°C, and after cooling, modified powder B is obtained; the modified powder B is sintered at 1500°C-1650°C, broken up, sieved, and the sieved material is taken to obtain artificial modified carbon;

[0009] The preparation method of granulated modified titanium-containing blast furnace slag is as follows: according to the mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100: (8-10): (3-6): (1-3), the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch are dry-milled to obtain ball-milled powder C; according to the mass ratio of ball-milled powder C: water: ZS-1071 high-temperature resistant inorganic binder = 100: (8-12): (1.5-3), water and ZS-1071 high-temperature resistant inorganic binder are added to the ball-milled powder C, the mixture is mixed evenly, briquette is pressed, sintered at 800°C-1000°C for 2h-3h, crushed after cooling, and classified to obtain granulated modified titanium-containing blast furnace slag.

[0010] In the preparation method of artificial modified carbon of the above technical solution, the stirring speed of the modification is 80rpm~120rpm, the modification time is 2h~3h; the sintering time is 4h~5h; the mesh number of the screening is 300 mesh~325 mesh.

[0011] In the method for preparing artificial modified carbon of the above technical solution, the powder structure of the modified powder B is that the surface of the particles of the calcined petroleum coke powder is coated with molybdenum disilicide and spinning pitch.

[0012] In the preparation method of granulated modified titanium-containing blast furnace slag of the above technical solution, the titanium content of the titanium-containing blast furnace slag is 22wt% to 26wt%; the median particle size of the titanium-containing blast furnace slag is 20μm to 40μm.

[0013] In the method for preparing granulated modified titanium-containing blast furnace slag of the above technical solution, the particle size range of boron carbide, diatomaceous earth and starch is all below 5 μm.

[0014] In the preparation method of the granulated modified titanium-containing blast furnace slag of the above technical solution, the dry ball milling time is 30 minutes to 40 minutes; water and ZS-1071 high temperature resistant inorganic binder are premixed before adding the ball milling powder C.

[0015] In the method for preparing granulated modified titanium-containing blast furnace slag of the above technical solution, the median particle size of the granulated modified titanium-containing blast furnace slag is 80 μm to 120 μm.

[0016] In the above technical solution, the particle size distribution of the dead-burned magnesium oxide is as follows: the particle size of 0.8mm to 3mm accounts for 65wt% to 75wt%, and the particle size of 0.075mm to 0.6mm accounts for 25wt% to 35wt%.

[0017] In the above technical solution, the calcination temperature of dead-burned magnesium oxide is 1800°C to 2000°C.

[0018] In the above technical solution, the phenolic resin is a thermosetting phenolic resin.

[0019] The method for preparing the above-mentioned thermal shock resistant and slag resistant magnesium carbon-based composite refractory brick comprises the following steps:

[0020] S1: mixing artificial modified carbon and granulated modified titanium-containing blast furnace slag uniformly by air flow according to their mass fractions to obtain mixed powder;

[0021] S2: Add the dead-burned magnesium oxide into the mixer according to the mass fraction, mix homogeneously for 3min to 5min, then add the phenolic resin and mix for 5min to 8min, finally add the mixed powder and mix for 10min to 15min, unload the material, press and form it in a brick press to obtain bricks, place the bricks in a drying kiln at 270℃ to 290℃ for heat treatment for 30h to 40h, and obtain refractory bricks after cooling.

[0022] In the above preparation method, the die pressure of compression molding is 250MPa to 280MPa.

[0023] The invention provides a heat-shock-resistant and slag-resistant magnesium-carbon-based composite refractory brick and a preparation method thereof, which has the following beneficial effects compared with the prior art:

[0024] 1. The refractory bricks of the present invention are prepared by using dead-burned magnesium oxide, artificial modified carbon, granulated modified titanium-containing blast furnace slag and phenolic resin. The artificial modified carbon and granulated modified titanium-containing blast furnace slag are easily homogeneously mixed with the dead-burned magnesium oxide, which can effectively reduce the uneven quality. During heat treatment, cracks caused by uneven thermal stress can be prevented, which can effectively improve the quality and qualified rate of the refractory bricks.

[0025] 2. The present invention adopts calcined petroleum coke powder, molybdenum disilicide powder and spinning pitch powder to mix in a specific ratio, and performs modification treatment at 360℃~450℃. By utilizing the adhesiveness of spinning pitch, nano-scale molybdenum disilicide powder and nano-scale spinning pitch powder can be evenly, densely and firmly coated on the surface of calcined petroleum coke powder particles to form a coating layer, which isolates and protects the calcined petroleum coke powder from surface oxidation during the subsequent carbonization treatment at 1500℃~1650℃, thereby improving the carbonization quality, having good oxidation resistance, ensuring the carbonization hardness of the particle material, and not causing The carbonaceous surface is oxidized and pulverized. It can ensure that when the refractory bricks are subsequently pressed, high-pressure molding of 250MPa to 280MPa can be achieved, thereby improving the density and strength of the brick body, and can reduce the oxidation reaction of the carbon surface and reduce thermal stress during high-temperature heat treatment at 270℃ to 290℃. When the refractory bricks are subsequently used, they maintain good performance and the artificial carbon components are not easily corroded and oxidized. The addition of carbon components can improve the thermal shock resistance while obtaining better strength, oxidation resistance and slag corrosion resistance, thereby extending the service life of the refractory bricks and reducing the impact on the furnace water components.

[0026] 3. The calcined petroleum coke coated particles are carbonized at 1500℃~1650℃ to obtain a molecular layer spacing morphology between hard carbon and graphite. The carbon layer spacing is smaller than hard carbon and larger than graphite, which means that it has good hardness, improves the strength, wear resistance and erosion resistance of refractory bricks, and can ensure the thermal shock resistance of refractory bricks in an environment of about 1600℃.

[0027] 4. The present invention uses titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch to mix in a specific proportion, and dry ball mill, so that the pores of the titanium-containing blast furnace slag particles are fully filled with boron carbide, diatomaceous earth and starch, and the water absorption expansion and adhesion of diatomaceous earth and starch are utilized to achieve the firmness of the pore filling; improve the particle structure of the titanium-containing blast furnace slag, effectively reduce the specific surface area of ​​the titanium-containing blast furnace slag particles, reduce the porosity of refractory bricks, and improve corrosion resistance; and the combination of titanium-containing blast furnace slag and boron carbide effectively improves oxidation resistance and corrosion resistance; in addition, it can also improve the compressive strength of the titanium blast furnace slag, thereby improving the compressive strength and wear resistance of the refractory bricks.

[0028] 5. After briquetting, crushing and granulation of titanium-containing blast furnace slag, boron carbide, diatomaceous earth, starch, water and ZS-1071 high-temperature resistant inorganic adhesive, the components can be more firmly combined and have good homogeneity. In the subsequent preparation of refractory bricks, it is easy to mix evenly, ensuring uniform thermal stress during heat treatment and no cracks caused by uneven thermal stress.

[0029] 6. After briquetting, materials such as titanium-containing blast furnace slag can be sintered at 800℃~1000℃ for 2h~3h to expel volatiles and carbonize some components, thereby increasing the granulation hardness, thermal shock resistance, compressive strength and high-temperature flexural strength.

[0030] 7. Titanium-containing blast furnace slag itself has good oxidation resistance. When it is combined with diatomite and boron carbide to prepare composite particles, its oxidation resistance can be further improved, thus extending the service life of refractory bricks.

[0031] 8. Adding ZS-1071 high temperature resistant inorganic adhesive for briquetting can make the components of the briquetting better bonded and not easy to pulverize. After crushing, it is not easy to produce a large amount of ultrafine powder, which can ensure that a suitable and concentrated particle size range is obtained, thereby improving the crushing yield. In addition, the granulated particles have good tightness and are not easy to disintegrate in the subsequent preparation process.

[0032] 9. The present invention adopts artificial modified carbon and granulated modified titanium-containing blast furnace slag for use. The homogeneity of each component material is good and the hardness is high. It can achieve compression molding at a pressure of 250MPa to 280MPa. It will not cause uneven thermal stress and thermal stress cracks when subjected to high-temperature heat treatment at 270℃ to 290℃, and can achieve the preparation of high-quality refractory bricks. The use of artificial modified carbon and granulated modified titanium-containing blast furnace slag can effectively improve the room-temperature compressive strength and high-temperature flexural strength of refractory bricks, and has outstanding thermal shock resistance and slag erosion resistance, which can greatly improve the thermal shock resistance and the ability to resist slag erosion, achieve a comprehensive improvement of various indicators, and extend the service life of refractory bricks. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with specific implementation cases, but the present invention is not limited to these embodiments.

[0034] Example 1: A heat-shock-resistant and slag-resistant magnesium-carbon-based composite refractory brick, the refractory brick comprising the following raw materials in parts by mass: 75 parts of dead-burned magnesium oxide, 12 parts of artificial modified carbon, 6.5 parts of granulated modified titanium-containing blast furnace slag, and 4 parts of phenolic resin; the particle size grading of the dead-burned magnesium oxide is as follows: the particle size of 0.8mm to 3mm accounts for 70wt%, and the particle size of 0.075mm to 0.6mm accounts for 30wt%; the calcination temperature of the dead-burned magnesium oxide is 1900°C; the phenolic resin is a thermosetting phenolic resin.

[0035] Among them, the preparation method of artificial modified carbon is: according to the mass ratio, calcined petroleum coke powder: molybdenum disilicide powder: spinning asphalt powder = 100:4:2.2, calcined petroleum coke powder with a median particle size of 12.6μm, nano-scale molybdenum disilicide powder and nano-scale spinning asphalt powder are evenly mixed by air flow to obtain mixed powder A; the mixed powder A is placed in a reactor and modified at 380°C. The modified stirring speed is 100rpm, and the modification time is 2.5h. After cooling, modified powder B is obtained. The powder structure of modified powder B is that the particle surface of calcined petroleum coke powder is coated with molybdenum disilicide and spinning asphalt; modified powder B is sintered at 1600°C for 4.5h, broken up, sieved through 325 mesh, and the sieved material is taken to obtain artificial modified carbon.

[0036] The preparation method of granulated modified titanium-containing blast furnace slag is as follows: take titanium-containing blast furnace slag with a titanium content of 23.6wt% and a median particle size of 26.5μm, take boron carbide, diatomaceous earth and starch with a particle size range of less than 5μm; according to the mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:9:5:2, dry ball mill the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch for 35min to obtain ball-milled powder C; according to the ball-milled powder C: The mass ratio of water: ZS-1071 high temperature resistant inorganic binder = 100:10:2.3. First, premix water and ZS-1071 high temperature resistant inorganic binder evenly to obtain a mixed solution. Then add the mixed solution of water and ZS-1071 high temperature resistant inorganic binder to the ball milled powder C, mix evenly, press into blocks, sinter at 900°C for 2.5h, crush and grade after cooling to obtain granulated modified titanium-containing blast furnace slag with a median particle size of 86.4μm.

[0037] The method for preparing the above-mentioned thermal shock resistant and slag resistant magnesium carbon-based composite refractory brick comprises the following steps:

[0038] S1: mixing artificial modified carbon and granulated modified titanium-containing blast furnace slag uniformly by air flow according to their mass fractions to obtain mixed powder;

[0039] S2: Add heavy burned magnesium oxide into a mixer according to the mass fraction, mix homogeneously for 4 minutes, then add phenolic resin and mix for 6 minutes, finally add mixed powder and mix for 12 minutes, unload the material, press and form it in a brick press with a die pressure of 260 MPa to obtain bricks, place the bricks in a drying kiln at 280°C for heat treatment for 35 hours, and obtain refractory bricks after cooling.

[0040] Example 2: A heat-shock-resistant and slag-resistant magnesium-carbon-based composite refractory brick, the refractory brick comprising the following raw materials in parts by mass: 70 parts of dead-burned magnesium oxide, 10 parts of artificial modified carbon, 5 parts of granulated modified titanium-containing blast furnace slag, and 3 parts of phenolic resin; the particle size grading of the dead-burned magnesium oxide is as follows: the particle size of 0.8mm to 3mm accounts for 65wt%, and the particle size of 0.075mm to 0.6mm accounts for 35wt%; the calcination temperature of the dead-burned magnesium oxide is 1800°C; the phenolic resin is a thermosetting phenolic resin.

[0041] Among them, the preparation method of artificial modified carbon is: according to the mass ratio, calcined petroleum coke powder: molybdenum disilicide powder: spinning asphalt powder = 100:3:1.5, calcined petroleum coke powder with a median particle size of 10.0 μm, nano-scale molybdenum disilicide powder and nano-scale spinning asphalt powder are evenly mixed by air flow to obtain mixed powder A; the mixed powder A is placed in a reactor and modified at 360°C. The modified stirring speed is 80 rpm, the modification time is 2 hours, and after cooling, modified powder B is obtained. The powder structure of modified powder B is that the particle surface of calcined petroleum coke powder is coated with molybdenum disilicide and spinning asphalt; the modified powder B is sintered at 1500°C for 4 hours, broken up, sieved with 300 mesh, and the sieved material is taken to obtain artificial modified carbon.

[0042] The preparation method of granulated modified titanium-containing blast furnace slag is as follows: take titanium-containing blast furnace slag with a titanium content of 22wt% and a median particle size of 20.0μm, take boron carbide, diatomaceous earth and starch with a particle size range of less than 5μm; according to the mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:8:3:1, dry ball mill the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch for 30min to obtain ball-milled powder C; according to the ball-milled powder C : water: ZS-1071 high temperature resistant inorganic binder = 100:8:1.5 mass ratio, first premix water and ZS-1071 high temperature resistant inorganic binder evenly to obtain a mixed solution, then add the mixed solution of water and ZS-1071 high temperature resistant inorganic binder to the ball milled powder C, mix evenly, press into blocks, sinter at 800°C for 2h, crush and grade after cooling, and obtain granulated modified titanium-containing blast furnace slag with a median particle size of 86.7μm.

[0043] The method for preparing the above-mentioned thermal shock resistant and slag resistant magnesium carbon-based composite refractory brick comprises the following steps:

[0044] S1: mixing artificial modified carbon and granulated modified titanium-containing blast furnace slag uniformly by air flow according to their mass fractions to obtain mixed powder;

[0045] S2: Add heavy burned magnesium oxide into a mixer according to the mass fraction, mix homogeneously for 3 minutes, then add phenolic resin and mix for 5 minutes, finally add mixed powder and mix for 10 minutes, unload the material, press and form it in a brick press with a die pressure of 250 MPa to obtain bricks, place the bricks in a drying kiln at 270°C for heat treatment for 30 hours, and obtain refractory bricks after cooling.

[0046] Example 3: A heat-shock-resistant and slag-resistant magnesium-carbon-based composite refractory brick, the refractory brick comprising the following raw materials in parts by mass: 78 parts of dead-burned magnesium oxide, 13 parts of artificial modified carbon, 7 parts of granulated modified titanium-containing blast furnace slag, and 4.5 parts of phenolic resin; the particle size grading of the dead-burned magnesium oxide is as follows: the particle size of 0.8mm to 3mm accounts for 72wt%, and the particle size of 0.075mm to 0.6mm accounts for 28wt%; the calcination temperature of the dead-burned magnesium oxide is 1950°C; the phenolic resin is a thermosetting phenolic resin.

[0047] Among them, the preparation method of artificial modified carbon is: according to the mass ratio, calcined petroleum coke powder: molybdenum disilicide powder: spinning asphalt powder = 100:4.5:2.2, calcined petroleum coke powder with a median particle size of 25.0 μm, nano-scale molybdenum disilicide powder and nano-scale spinning asphalt powder are evenly mixed by air flow to obtain mixed powder A; the mixed powder A is placed in a reactor and modified at 420°C. The modified stirring speed is 110 rpm, the modification time is 3 hours, and after cooling, modified powder B is obtained. The powder structure of modified powder B is that the particle surface of calcined petroleum coke powder is coated with molybdenum disilicide and spinning asphalt; the modified powder B is sintered at 1600°C for 4.5 hours, broken up, sieved with 325 mesh, and the sieved material is taken to obtain artificial modified carbon.

[0048] The preparation method of granulated modified titanium-containing blast furnace slag is as follows: take titanium-containing blast furnace slag with a titanium content of 25wt% and a median particle size of 36.2μm, take boron carbide, diatomaceous earth and starch with a particle size range of less than 5μm; according to the mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:9.5:5:2.5, dry-mill the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch for 38min to obtain ball-milled powder C; according to the mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:9.5:5:2.5, dry-mill the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch for 38min to obtain ball-milled powder C; C: water: ZS-1071 high temperature resistant inorganic binder = mass ratio of 100:11:2.5. First, premix water and ZS-1071 high temperature resistant inorganic binder evenly to obtain a mixed solution. Then add the mixed solution of water and ZS-1071 high temperature resistant inorganic binder to the ball milled powder C, mix evenly, press into blocks, sinter at 950°C for 3h, crush and grade after cooling to obtain granulated modified titanium-containing blast furnace slag with a median particle size of 80.0μm.

[0049] The method for preparing the above-mentioned thermal shock resistant and slag resistant magnesium carbon-based composite refractory brick comprises the following steps:

[0050] S1: mixing artificial modified carbon and granulated modified titanium-containing blast furnace slag uniformly by air flow according to their mass fractions to obtain mixed powder;

[0051] S2: Add heavy burned magnesium oxide into a mixer according to the mass fraction, mix homogeneously for 4 minutes, then add phenolic resin and mix for 7 minutes, finally add mixed powder and mix for 14 minutes, unload the material, press and form it in a brick press with a die pressure of 270 MPa to obtain bricks, place the bricks in a drying kiln at 285°C for heat treatment for 36 hours, and obtain refractory bricks after cooling.

[0052] Example 4: A heat-shock-resistant and slag-resistant magnesium-carbon-based composite refractory brick, the refractory brick comprising the following raw materials in parts by mass: 80 parts of dead-burned magnesium oxide, 15 parts of artificial modified carbon, 8 parts of granulated modified titanium-containing blast furnace slag, and 5 parts of phenolic resin; the particle size grading of the dead-burned magnesium oxide is as follows: the particle size of 0.8mm to 3mm accounts for 75wt%, and the particle size of 0.075mm to 0.6mm accounts for 25wt%; the calcination temperature of the dead-burned magnesium oxide is 2000°C; the phenolic resin is a thermosetting phenolic resin.

[0053] Among them, the preparation method of artificial modified carbon is: according to the mass ratio, calcined petroleum coke powder: molybdenum disilicide powder: spinning asphalt powder = 100:5:2.5, calcined petroleum coke powder with a median particle size of 18.4μm, nano-scale molybdenum disilicide powder and nano-scale spinning asphalt powder are evenly mixed by air flow to obtain mixed powder A; the mixed powder A is placed in a reactor and modified at 450°C. The modified stirring speed is 120rpm, the modification time is 3h, and after cooling, modified powder B is obtained. The powder structure of modified powder B is that the particle surface of calcined petroleum coke powder is coated with molybdenum disilicide and spinning asphalt; the modified powder B is sintered at 1650°C for 5h, broken up, sieved with 325 mesh, and the sieved material is taken to obtain artificial modified carbon.

[0054] The preparation method of granulated modified titanium-containing blast furnace slag is as follows: take titanium-containing blast furnace slag with a titanium content of 26wt% and a median particle size of 40.0μm, take boron carbide, diatomaceous earth and starch with a particle size range of less than 5μm; according to the mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:10:6:3, dry ball mill the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch for 40min to obtain ball-milled powder C; according to the ball-milled powder C : water: ZS-1071 high temperature resistant inorganic binder = 100:12:3 by mass ratio. First, premix water and ZS-1071 high temperature resistant inorganic binder evenly to obtain a mixed solution. Then add the mixed solution of water and ZS-1071 high temperature resistant inorganic binder to the ball milled powder C, mix evenly, press into blocks, sinter at 1000°C for 3h, crush and grade after cooling to obtain granulated modified titanium-containing blast furnace slag with a median particle size of 112.3μm.

[0055] The method for preparing the above-mentioned thermal shock resistant and slag resistant magnesium carbon-based composite refractory brick comprises the following steps:

[0056] S1: mixing artificial modified carbon and granulated modified titanium-containing blast furnace slag uniformly by air flow according to their mass fractions to obtain mixed powder;

[0057] S2: Add heavy burned magnesium oxide into a mixer according to the mass fraction, mix homogeneously for 5 minutes, then add phenolic resin and mix for 8 minutes, finally add mixed powder and mix for 15 minutes, unload the material, press and form it in a brick press with a die pressure of 280 MPa to obtain bricks, place the bricks in a drying kiln at 290°C for heat treatment for 40 hours, and obtain refractory bricks after cooling.

[0058] Example 5: A heat-shock-resistant and slag-resistant magnesium-carbon-based composite refractory brick, the refractory brick comprising the following raw materials in parts by mass: 72 parts of dead-burned magnesium oxide, 12 parts of artificial modified carbon, 6 parts of granulated modified titanium-containing blast furnace slag, and 3.5 parts of phenolic resin; the particle size grading of the dead-burned magnesium oxide is as follows: the particle size of 0.8mm to 3mm accounts for 68wt%, and the particle size of 0.075mm to 0.6mm accounts for 32wt%; the calcination temperature of the dead-burned magnesium oxide is 1850°C; the phenolic resin is a thermosetting phenolic resin.

[0059] Among them, the preparation method of artificial modified carbon is: according to the mass ratio, calcined petroleum coke powder: molybdenum disilicide powder: spinning asphalt powder = 100:3.5:2.0, calcined petroleum coke powder with a median particle size of 15.7μm, nano-scale molybdenum disilicide powder and nano-scale spinning asphalt powder are evenly mixed by air flow to obtain mixed powder A; mixed powder A is placed in a reactor and modified at 380°C. The modified stirring speed is 90rpm, the modification time is 2h, and after cooling, modified powder B is obtained. The powder structure of modified powder B is that the particle surface of calcined petroleum coke powder is coated with molybdenum disilicide and spinning asphalt; modified powder B is sintered at 1550°C for 4h, broken up, sieved with 300 mesh, and the sieved material is taken to obtain artificial modified carbon.

[0060] The preparation method of granulated modified titanium-containing blast furnace slag is as follows: take titanium-containing blast furnace slag with a titanium content of 23wt% and a median particle size of 32.1μm, take boron carbide, diatomaceous earth and starch with a particle size range of less than 5μm; according to the mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:8.5:4:1.5, dry-mill the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch for 32min to obtain ball-milled powder C; according to the ball milling The mass ratio of powder C: water: ZS-1071 high temperature resistant inorganic binder = 100:9:2. First, premix water and ZS-1071 high temperature resistant inorganic binder evenly to obtain a mixed solution, and then add the mixed solution of water and ZS-1071 high temperature resistant inorganic binder to the ball milled powder C, mix evenly, press into blocks, sinter at 850°C for 2h, crush and grade after cooling to obtain granulated modified titanium-containing blast furnace slag with a median particle size of 120.0μm.

[0061] The method for preparing the above-mentioned thermal shock resistant and slag resistant magnesium carbon-based composite refractory brick comprises the following steps:

[0062] S1: mixing artificial modified carbon and granulated modified titanium-containing blast furnace slag uniformly by air flow according to their mass fractions to obtain mixed powder;

[0063] S2: Add heavy burned magnesium oxide into a mixer according to the mass fraction, mix homogeneously for 3 minutes, then add phenolic resin and mix for 6 minutes, finally add mixed powder and mix for 10 minutes, unload the material, press and form it in a brick press with a die pressure of 260 MPa to obtain bricks, place the bricks in a drying kiln at 275°C for heat treatment for 32 hours, and obtain refractory bricks after cooling.

[0064] The ZS-1071 high temperature resistant inorganic adhesive used in the above embodiments is made of inorganic nano materials through polycondensation reaction, does not contain harmful volatile organic compounds, is non-corrosive to metal substrates, and has strong bonding strength; it is produced by Beijing Zhisheng Weihua Chemical Co., Ltd.

[0065] Comparative Example 1: No artificial modified carbon was prepared, and the artificial modified carbon component was replaced by natural graphite powder and molybdenum disilicide powder, with a mass ratio of natural graphite powder: molybdenum disilicide powder = 100:4. Other parameters and methods were the same as in Example 1.

[0066] Comparative Example 2: Instead of preparing granulated modified titanium-containing blast furnace slag, the granulated modified titanium-containing blast furnace slag was replaced by titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch, with a mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:9:5:2. Other parameters and methods were the same as in Example 1.

[0067] Comparative Example 3: Instead of preparing granulated modified titanium-containing blast furnace slag, the granulated modified titanium-containing blast furnace slag is replaced by titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch, with a mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:9:5:2; in the preparation method, the die head pressure is 180 MPa, bricks are obtained, and the bricks are placed in a drying kiln at 240°C for heat treatment for 35 hours to obtain refractory bricks. Other parameters and methods are the same as in Example 1.

[0068] Comparative Example 4: No artificial modified carbon is prepared, and the artificial modified carbon component is replaced by natural graphite powder and molybdenum disilicide powder, and the mass ratio is natural graphite powder: molybdenum disilicide powder = 100:4; granulated modified titanium-containing blast furnace slag is not prepared, and the granulated modified titanium-containing blast furnace slag component is replaced by titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch, and the mass ratio is titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:9:5:2. Other parameters and methods are the same as in Example 1.

[0069] Comparative Example 5: No artificial modified carbon is prepared, and the artificial modified carbon component is replaced by natural graphite powder and molybdenum disilicide powder, and the mass ratio is natural graphite powder: molybdenum disilicide powder = 100:4; granulated modified titanium-containing blast furnace slag is not prepared, and the granulated modified titanium-containing blast furnace slag component is replaced by titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch, and the mass ratio is titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100:9:5:2; in the preparation method, the die pressure is 180MPa, and bricks are obtained. The bricks are placed in a drying kiln at 240°C for heat treatment for 35h and then cooled to obtain refractory bricks. Other parameters and methods are the same as in Example 1.

[0070] Comparative Example 6: Refractory brick composition: 75 parts of dead-burned magnesium oxide, 12 parts of natural graphite, 6.5 parts of titanium-containing blast furnace slag, 1.5 parts of boron carbide, and 4 parts of phenolic resin; in the preparation method, the die pressure is 180 MPa to obtain bricks, and the bricks are placed in a drying kiln at 240°C for heat treatment for 35 hours and then cooled to obtain refractory bricks. Other parameters and methods are the same as in Example 1.

[0071] The refractory bricks of the above embodiments and comparative examples were made into test sample sizes and subjected to the following performance tests:

[0072] Performance testing is carried out in accordance with "Magnesium Carbon Brick" GB / T 22589-2017 and related testing specifications. The room temperature compressive strength test specimen specifications are: 50mm cube; high temperature flexural strength test specimen specifications are: 150mm×25mm×25mm strip, test conditions: 1400℃×0.5h. Refractory bricks are prepared into 114mm×64mm×64mm strip specimens for thermal shock resistance testing, test conditions: 1400℃×0.5h·air cooling. Slag resistance performance testing is carried out in accordance with "Refractories Slag Resistance Test Method" GB / T 8931-2007: Refractory bricks are prepared into crucible specimen specifications, with an outer dimension of 70mm 3 , inner size specification, φ40mm×35mm, filled with steel slag, furnace temperature 1650℃, keep warm for 10min, repeat 5 times. 5 parallel samples are tested for each type, and the average value is taken. The results are shown in Table 1 below:

[0073] Table 1 Performance test results of refractory bricks

[0074]

[0075] Among them, the refractory bricks of Comparative Examples 2 and 4 were prepared in 50 mm cubes. The bricks were placed in a drying kiln at 280° C. for heat treatment for 35 hours. Thermal stress cracks occurred after leaving the kiln. The refractory bricks were unqualified and could not be tested in all subsequent tests.

[0076] By comparing the test results of Examples 1 to 5 with those of Comparative Example 6, it can be seen that the refractory bricks of Examples 1 to 5 have excellent room-temperature compressive strength and high-temperature flexural strength, and outstanding thermal shock resistance and slag erosion resistance, and can greatly improve the thermal shock resistance and the ability to resist slag erosion, and the comprehensive performance is significantly improved, the service life is extended, the erosion rate is low, and the impact on the composition of boiler water can be effectively reduced.

[0077] From Comparative Examples 2 and 4, it can be seen that the refractory bricks formed by die pressure of 250MPa or more in Examples 1 to 5 can be heat treated at 270°C or above without thermal stress cracking, and have good crack resistance; that is, the granulated modified titanium-containing blast furnace slag has a good effect of resisting thermal stress cracking. In Comparative Examples 2 and 4, granulated modified titanium-containing blast furnace slag is not prepared, and after high pressure forming, heat treatment is performed at 270°C or above, thermal stress cracking occurs, and qualified refractory bricks cannot be obtained.

[0078] It can be seen from the test results of Comparative Example 1 that no artificial modified carbon is prepared, that is, the artificial modified carbon component is replaced by natural graphite powder and molybdenum disilicide powder, and there is no antioxidant protective layer on the surface of the carbon component particles. The carbon component is easily oxidized, and the material bonding, high-temperature flexural strength, thermal shock resistance, and slag resistance will be reduced. The refractory brick components, especially the carbon components, will penetrate into the furnace water and affect the furnace water composition.

[0079] It can be seen from the test results of Comparative Example 3 that if the granulated modified titanium-containing blast furnace slag is not prepared, and the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch are not subjected to high-temperature sintering and granulation treatment, the room-temperature compressive strength and high-temperature flexural strength of the refractory bricks will be greatly affected, and the thermal shock resistance and slag erosion resistance are also poor. On the one hand, this is because the molding pressure, heat treatment temperature and density are low when preparing refractory bricks, which cannot achieve high room-temperature compressive strength and high-temperature flexural strength, and the wear resistance is poor, resulting in poor slag erosion resistance; on the other hand, it is difficult to improve the various performances of refractory bricks due to the uneven dispersion of the components, poor bonding of the components and uneven quality.

[0080] It can be seen from the test results of Example 1 and Comparative Example 5 that the combination of artificial modified carbon and granulated modified titanium-containing blast furnace slag has a good synergistic effect and can significantly improve the various properties of refractory bricks.

Claims

1. A thermal shock and slag resistant magnesium carbon based composite refractory brick, characterized in that: The refractory bricks include the following raw materials in parts by weight: 70 to 80 parts of dead-burned magnesium oxide, 10 to 15 parts of artificial modified carbon, 5 to 8 parts of granulated modified titanium-containing blast furnace slag, and 3 to 5 parts of phenolic resin; The preparation method of the artificial modified carbon is as follows: according to the mass ratio of calcined petroleum coke powder: molybdenum disilicide powder: spinning pitch powder = 100: (3-5): (1.5-2.5), calcined petroleum coke powder with a median particle size of 10 μm to 25 μm, nano-scale molybdenum disilicide powder and nano-scale spinning pitch powder are evenly mixed by air flow to obtain mixed powder A; the mixed powder A is placed in a reaction kettle, modified at 360° C. to 450° C., and after cooling, modified powder B is obtained; the modified powder B is sintered at 1500° C. to 1650° C., broken up, sieved, and the sieved material is taken to obtain artificial modified carbon; The preparation method of the granulated modified titanium-containing blast furnace slag comprises the following steps: dry-milling the titanium-containing blast furnace slag, boron carbide, diatomaceous earth and starch according to the mass ratio of titanium-containing blast furnace slag: boron carbide: diatomaceous earth: starch = 100: (8-10): (3-6): (1-3) to obtain ball mill powder C; adding water and ZS-1071 high temperature resistant inorganic binder to the ball mill powder C according to the mass ratio of ball mill powder C: water: ZS-1071 high temperature resistant inorganic binder = 100: (8-12): (1.5-3), mixing evenly, pressing into blocks, sintering at 800-1000° C. for 2-3 hours, crushing after cooling, and classifying to obtain the granulated modified titanium-containing blast furnace slag.

2. The thermal shock and slag resistant magnesium carbon based composite refractory brick according to claim 1, characterized in that: In the preparation method of artificial modified carbon, the stirring speed of the modification is 80rpm-120rpm, the modification time is 2h-3h; the sintering time is 4h-5h; the mesh number of the screening is 300-325 mesh.

3. The thermal shock and slag resistant magnesium carbon based composite refractory brick according to claim 1, characterized in that: In the method for preparing artificial modified carbon, the powder structure of the modified powder B is that the surface of the particles of the calcined petroleum coke powder is coated with molybdenum disilicide and spinning pitch.

4. The thermal shock and slag resistant magnesium carbon based composite refractory brick according to claim 1, characterized in that: In the preparation method of granulated modified titanium-containing blast furnace slag, the titanium content of the titanium-containing blast furnace slag is 22wt% to 26wt%; the median particle size of the titanium-containing blast furnace slag is 20μm to 40μm.

5. The thermal shock and slag resistant magnesium carbon based composite refractory brick according to claim 1, characterized in that: In the method for preparing granulated modified titanium-containing blast furnace slag, the particle sizes of the boron carbide, diatomaceous earth and starch are all below 5 μm.

6. The thermal shock and slag resistant magnesium carbon based composite refractory brick according to claim 1, characterized in that: In the preparation method of granulated modified titanium-containing blast furnace slag, the dry ball milling time is 30 minutes to 40 minutes; the water and ZS-1071 high temperature resistant inorganic binder are premixed uniformly before being added into the ball milling powder C.

7. The thermal shock and slag resistant magnesium carbon based composite refractory brick according to claim 1, characterized in that: In the preparation method of granulated modified titanium-containing blast furnace slag, the median particle size of the granulated modified titanium-containing blast furnace slag is 80 μm to 120 μm.

8. The thermal shock and slag resistant magnesium carbon based composite refractory brick according to claim 1, characterized in that: The particle size distribution of the dead-burned magnesium oxide is as follows: the particle size of 0.8mm to 3mm accounts for 65wt% to 75wt%, and the particle size of 0.075mm to 0.6mm accounts for 25wt% to 35wt%; the calcination temperature of the dead-burned magnesium oxide is 1800°C to 2000°C; and the phenolic resin is a thermosetting phenolic resin.

9. The method for preparing the thermal shock and slag resistant magnesium carbon based composite refractory bricks according to claim 1, characterized in that: The steps include: S1: mixing artificial modified carbon and granulated modified titanium-containing blast furnace slag uniformly by air flow according to their mass fractions to obtain mixed powder; S2: Add the dead-burned magnesium oxide into the mixer according to the mass fraction, mix homogeneously for 3min to 5min, then add the phenolic resin and mix for 5min to 8min, finally add the mixed powder and mix for 10min to 15min, unload the material, press and form it in a brick press to obtain bricks, place the bricks in a drying kiln at 270℃ to 290℃ for heat treatment for 30h to 40h, and obtain refractory bricks after cooling.

10. The method for preparing a thermal shock and slag resistant magnesium carbon based composite refractory brick according to claim 9, characterized in that: The die head pressure of the compression molding is 250MPa to 280MPa.

Citation Information

Cited By

  • Magnesia-carbon refractory material with high thermal shock resistance and erosion resistance and preparation method thereof

    CN120794578A

  • High-erosion-resistance refractory brick and production process thereof

    CN121850617A