PVA-CA / polyfluorene-copper oxide nanofiber composite membrane and its preparation method and application

Through the preparation of PVA-CA/polyfluorene-copper oxide nanofiber composite film, the electrospinning method and the characteristics of semiconductor materials are used to solve the problem of poor ethylene degradation and bactericidal effect in fruits and vegetables preservation in the prior art, and achieve the goal of achieving Functional and environmentally friendly packaging materials.

CN118668384BActive Publication Date: 2024-11-22SHANDONG BOBANG TAISHENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411139090.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The existing fresh-preserving packaging products have problems such as single functions, unstable insulation effect, poor degradability, wide catalyst band gap and low electron mobility in the preservation of fruits and vegetables, making it difficult to achieve ethylene degradation and sterilization effects at the same time.

Method used

The preparation method of PVA-CA/polyfluorene-copper oxide nanofiber composite film is adopted to prepare the nanofiber composite film by electrospinning, and the semiconductor characteristics of polyfluorene and copper oxide are used to achieve ethylene degradation and bactericidal functions under visible light.

Benefits of technology

It realizes excellent ethylene degradation and bactericidal function under visible light conditions, improves electron mobility and bactericidal ability, and has uniform and stable membrane performance, which is suitable for the preservation of fruits and vegetables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118668384B_ABST
    Figure CN118668384B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of preparation and application of nanomaterials, and specifically relates to a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane and a preparation method and application thereof. The preparation method of the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane comprises the following steps: adding polyfluorene-copper oxide to a PVA solution to obtain a PVA / polyfluorene-copper oxide solution, adding citric acid to obtain a PVA-CA / polyfluorene-copper oxide solution; and using an electrostatic spinning film-forming method to prepare a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane from the PVA-CA / polyfluorene-copper oxide solution. The preparation method of the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane provided by the present invention, the prepared composite membrane has excellent ethylene degradation function and sterilization function, and the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane prepared by the present invention is mainly used in the preservation of fruits and vegetables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation and application of nano materials, and specifically relates to a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane and a preparation method and application thereof. Background Art

[0002] Due to microbial infection, environmental factors and storage conditions, fruits and vegetables suffer serious losses during the storage period after picking. On the one hand, fruits and vegetables will produce ethylene during storage, and low concentrations (0.01-0.1mL / L) of ethylene will catalyze the fruit, but after the storage period is extended, most fruits and vegetables will become highly aged and perishable. On the other hand, microbial infection causes serious losses of fruits and vegetables. In order to reduce losses, most of them are packaged for freshness preservation.

[0003] However, most of the current fresh-keeping packaging products rely on cooling to achieve the heat preservation function. Not only are the functions single, but the heat preservation effect is unstable. Therefore, the achieved fresh-keeping effect is not ideal and cannot solve the fundamental problem. In addition, most fresh-keeping packaging products are fresh-keeping films, which have poor degradability and are not environmentally friendly. Therefore, there are improvements to nanofiber composite membranes in the prior art. For example, CN103103696A discloses a preparation and application of a biologically active antibacterial nanofiber composite membrane, in which lysozyme and EDTA are added to a polyvinyl alcohol solution; spinning and vacuum drying are performed to obtain a biologically active antibacterial nanofiber composite membrane. By adding lysozyme, the prepared composite membrane achieves an antibacterial effect. The conditions for adding lysozyme are relatively mild, and it is easily destroyed during processing. The antibacterial effect is not obvious and the duration is short. For example, CN103266424A discloses a nanofiber composite film containing a plant-derived antibacterial agent, a preparation method and an application thereof, wherein β-cyclodextrin and cinnamon essential oil are sequentially added to a polyvinyl alcohol solution, and after electrostatic spinning and vacuum drying, a nanofiber composite film containing a plant-derived antibacterial agent is obtained, which has a good antibacterial effect. However, under high temperature and light conditions, after cyclodextrin is destroyed, the antibacterial effect is lost, and therefore the product is unstable. For example, CN1583871A discloses an enhanced polyvinyl alcohol composite film and a preparation method and use thereof, wherein a nano titanium dioxide aqueous solution is added to a polyvinyl alcohol solution, a film is prepared by a blending method, and dried to obtain an enhanced polyvinyl alcohol composite film. Although the prepared composite film has bactericidal and degradable properties, its bactericidal effect depends on the reaction of bacteria and titanium dioxide, and the bactericidal effect is unstable.

[0004] In addition, existing catalysts are not suitable for daily fruit and vegetable preservation. There are two main problems. First, the band gap of the selected materials is wide, the catalytic conditions are harsh, and only ultraviolet light can be used for catalysis; second, the electron mobility is too low, resulting in a short electron hole existence time and low catalytic efficiency. Therefore, in the field of photocatalysis, composite membranes that can simultaneously perform sterilization and ethylene catalysis are urgently needed. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for preparing a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane. The prepared composite membrane has excellent ethylene degradation function and bactericidal function. The PVA-CA / polyfluorene-copper oxide nanofiber composite membrane prepared by the present invention is mainly used in the preservation of fruits and vegetables.

[0006] The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane of the present invention comprises the following steps:

[0007] (1) Dissolve PVA in water and stir at 80-90°C for 1.5-2h to obtain a PVA solution;

[0008] (2) adding polyfluorene-copper oxide to the PVA solution and stirring at 70-80° C. for 1.5-2 h to obtain a PVA / polyfluorene-copper oxide solution;

[0009] (3) Adding citric acid (CA) to the PVA / polyfluorene-copper oxide solution and reacting at room temperature for 1.5-2 hours to obtain a PVA-CA / polyfluorene-copper oxide solution;

[0010] (4) The PVA-CA / polyfluorene-copper oxide solution was subjected to electrospinning to prepare a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane.

[0011] The mass ratio of PVA to polyfluorene-copper oxide is (5:1)-(6:1).

[0012] The mass ratio of PVA to citric acid is (20:3)-(5:1).

[0013] The process parameters of the electrospinning in step (4) are: a stable flow rate of 0.24-0.26 mL / h, an applied voltage of 14.5-15 kV, and a pumping time of 1.5-2 h; the electrospinning uses a syringe with a DC power supply regulation, and the tip is 16-17 cm away from the collector.

[0014] The preparation method of polyfluorene-copper oxide comprises the following steps:

[0015] (1) dissolving polyfluorene in water to obtain a polyfluorene solution;

[0016] (2) Copper acetate Cu(CH 3 COO 2 ·H 2 O was dissolved in distilled water, and then the polyfluorene solution was added;

[0017] (3) Continue to drip ammonia water, stir for 30-40 minutes, then add alkali to maintain the pH at 10.5-11, stir for 30-60 minutes, and obtain a homogeneous solution; the ammonia water is added first to react with the copper acetate to replace the acetate ion, which is beneficial to the subsequent formation of copper oxide and prevents the direct formation of iron hydroxide precipitation during the direct addition of alkali, and forms copper oxide crystals on the polyfluorene under the hydrothermal reaction;

[0018] (4) subjecting the homogeneous solution to a hydrothermal reaction at 180-200°C for 24-32 hours, and washing to obtain a black precipitate;

[0019] (5) Dry the black precipitate at 50-60°C for 12-16 hours to obtain polyfluorene-copper oxide.

[0020] Copper acetateCu(CH 3 COO 2 ·H 2 The molar ratio of O to ammonia water is 1:(1.2-1.5).

[0021] The base is NaOH or KOH.

[0022] Polyfluorene and copper acetate Cu(CH 3 COO 2 ·H 2 The mass ratio of O is 1:(1.13-1.26).

[0023] A PVA-CA / polyfluorene-copper oxide nanofiber composite membrane is prepared by the preparation method of the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane.

[0024] Application of a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane: used in the preservation of fruits and vegetables, with antibacterial and ethylene removal functions.

[0025] Specifically, the method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane comprises the following steps:

[0026] (1) Preparation of polyfluorene-copper oxide:

[0027] a. Dissolve polyfluorene in water to obtain a polyfluorene solution.

[0028] b. Dissolve copper acetate in distilled water and then add the polyfluorene solution.

[0029] c. Continue to slowly drip in ammonia water, stir for 30-40 minutes, then add NaOH or KOH to maintain the pH at 10.5-11, stir for 30-60 minutes to obtain a homogeneous solution; adding ammonia water first is to react with copper acetate to replace acetate ions, which is beneficial to the subsequent formation of copper oxide and prevents the direct formation of iron hydroxide precipitation during the direct addition of alkali. Copper oxide crystals are formed on the polyfluorene under the hydrothermal reaction; the molar ratio of copper acetate to ammonia water is 1: (1.2-1.5).

[0030] d. The homogeneous solution is subjected to hydrothermal reaction at 180-200°C for 24-32 hours, and a black precipitate is obtained after washing.

[0031] e. Dry the black precipitate in an oven at 50-60°C for 12-16 hours to obtain polyfluorene-copper oxide.

[0032] (2) Dissolve PVA in water and stir at 80-90°C for 1.5-2h to obtain a PVA solution;

[0033] (3) Add polyfluorene-copper oxide to the PVA solution and stir at 70-80° C. for 1.5-2 h to obtain a PVA / polyfluorene-copper oxide solution; the mass ratio of PVA to polyfluorene-copper oxide is (5:1)-(6:1).

[0034] (4) Add citric acid (CA) to the PVA / polyfluorene-copper oxide solution, and stir the mixture at room temperature for 1.5-2 hours to obtain a PVA-CA / polyfluorene-copper oxide solution; the mass ratio of PVA to citric acid is (20:3)-(5:1).

[0035] (5) The PVA-CA / polyfluorene-copper oxide solution was transferred to a 10 mL syringe with a voltage-regulated DC power supply, with the tip 16-17 cm away from the collector. The solution was pumped at a steady flow rate of 0.24-0.26 mL / h and an applied voltage of 14.5-15 kV for 1.5-2 h by electrospinning, and then collected to obtain the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane.

[0036] The preparation method of the polyfluorene comprises the following steps:

[0037] (a) A mixture of 2,7-dibromofluorene, tetrabutylammonium bromide, 1,3-dibromopropane and sodium hydroxide aqueous solution was heated to 70°C, refluxed for 8 h, cooled to room temperature, extracted with dichloromethane, and the organic phase was washed three times with distilled water and once with saturated brine. 2 SO 4 After drying, dichloromethane was removed, and then excess 1,3-dibromopropane was removed under reduced pressure. The residual material was separated by column to obtain a white powdery solid (triethoxyphosphine of 2,7-dibromo-9,9-di(3-bromopropyl)fluorene).

[0038] (b) The triethoxyphosphorus solution of 2,7-dibromo-9,9-di(3-bromopropyl)fluorene was heated to 140°C and refluxed for 16 hours. After the reaction was completed, the solution was cooled and the excess triethoxyphosphorus was evaporated under reduced pressure. The residual material was separated using a neutral alumina column, and impurities were removed using an eluent of ethyl acetate / petroleum ether = 1:1. Ethyl acetate was then used as the eluent to obtain white granular microcrystals (2,7-dibromo-9,9-di(3-phosphoethylpropyl)fluorene).

[0039] (c) 2,7-Dibromo-9,9-bis(3-phosphoethylpropyl)fluorene was dissolved in dichloromethane, and trimethylsilyl bromide was added dropwise under argon protection. After the addition was complete, the reaction was carried out at room temperature for 10 hours. After the reaction was completed, the excess trimethylsilyl bromide and dichloromethane were removed under reduced pressure. The residual material was dissolved in methanol. After stirring at room temperature for 6 hours, the methanol was removed under reduced pressure again to obtain a light yellow solid. The solid was ultrasonically washed with water until white and then dried in vacuo at 50°C for 12 hours to obtain a white powdery solid (2,7-dibromo-9,9-bis(3-phosphopropyl)fluorene).

[0040] (d) Under argon protection, 2,7-dibromo-9,9-di(3-phosphopropyl)fluorene, 1,4-phenylenediboronic acid bis(pinacol) ester, and Pd(dppf)Cl were added to the reaction bottle connected to the double-row tube. 2 , N,N-dimethylformamide and 2M Na 2 CO 3 Aqueous solution, under argon protection, stirred and reacted at 85°C for 60 hours, phenylboric acid was dissolved in N,N-dimethylformamide, the air was exhausted for 30 minutes after ventilation, and the reaction was introduced into a reaction bottle for 5 hours. Bromobenzene was added to the reaction bottle and reacted for another 5 hours. After the reaction was completed, the reaction solution was injected into cold acetone, and the precipitated solid was filtered and vacuum dried and then dissolved in distilled water again. The solution was dialyzed through a dialysis membrane for 3 days, and the water was changed every 6 hours. After the dialysis was completed, the solution in the dialysis membrane was concentrated and precipitated in acetone again. After filtration and vacuum drying, a dark yellow powdery solid was obtained, namely polyfluorene.

[0041] The reaction equation of polyfluorene is as follows Figure 1 shown.

[0042] The PVA-CA reaction formula prepared by the present invention is as follows: Figure 2 shown.

[0043] The present invention uses a polyfluorene / copper oxide composite material and PVA to be composited by cross-linking, and then uses an electrostatic spinning method to prepare a composite membrane. The prepared PVA-CA / polyfluorene-copper oxide nanofiber composite membrane uses polyfluorene, which is an n-type semiconductor material, and copper oxide, which is a p-type semiconductor material. Under the excitation of visible light, the free electrons in the valence band absorb photon energy and transition to the conduction band, while leaving the same number of holes in its valence band. The matching band structures of polyfluorene and copper oxide form a "step", and the photogenerated electrons move to the conduction band of copper oxide, while the holes gather in the valence band of polyfluorene, thereby greatly reducing the recombination rate of electrons and holes. The photogenerated electrons that move to the surface of the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane combine with the dissolved oxygen adsorbed on the surface of the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane to generate superoxide radicals (•O 2- ), while holes and OH - Reacts with water to form hydroxyl radicals (•OH - ), and further form H 2 O 2 •. 2- ,•OH - and H 2 O 2 They all have strong oxidizing properties, undergo redox reactions with the ethylene released by fruits and vegetables to generate water and carbon dioxide, and react with the membrane structure of bacteria to kill the bacteria.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] (1) The polyfluorene prepared in the present invention not only meets the wide band gap required for the catalysis of the PVA-CA / polyfluorene-copper oxide nanofiber composite film, but also solves the problem of electron mobility through the special heterojunction structure of the composite film, which enables the composite film to have excellent ethylene degradation and sterilization functions under visible light conditions.

[0046] (2) The method of the present invention firstly mixes the polyfluorene / copper oxide composite material with PVA. The phosphate groups contained in the polyfluorene play a role in cross-linking the PVA during the mixing process. At the same time, citric acid is mixed in to thoroughly cross-link and catalyze the PVA, so that the polyfluorene / copper oxide composite material grows together with the PVA body. This not only gives the PVA catalytic ability, but also, due to the existence of the electron sharing system, it will have electron holes that exist longer, thereby improving the bactericidal ability.

[0047] (3) The PVA-CA / polyfluorene-copper oxide nanofiber composite membrane prepared by the present invention adopts an electrospinning method to form the membrane, and the performance of the membrane is uniform and stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1is the reaction formula of the polyfluorene of the present invention.

[0049] Figure 2 This is the reaction formula for preparing PVA-CA of the present invention. DETAILED DESCRIPTION

[0050] The present invention will be further described below in conjunction with specific embodiments.

[0051] The raw materials or reagents used in the present invention are all normal commercially available products. The PVA used is PVA1799, and the ammonia water used is from Sinopharm Group Pharmaceutical Co., Ltd., with a mass concentration of 25%, a relative density of 0.91 g / mL (20° C.) relative to water, and a molar weight based on a molecular weight of 35.

[0052] The preparation method of the polyfluorene comprises the following steps:

[0053] (a) A mixture of 2,7-dibromofluorene, tetrabutylammonium bromide, 1,3-dibromopropane and sodium hydroxide aqueous solution was heated to 70°C, refluxed for 8 hours, cooled to room temperature, extracted with dichloromethane, and the organic phase was washed three times with distilled water and once with saturated brine. 2 SO 4 After drying, dichloromethane was removed, and then excess 1,3-dibromopropane was removed under reduced pressure. The residual material was separated by column to obtain a white powdery solid (triethoxyphosphine of 2,7-dibromo-9,9-di(3-bromopropyl)fluorene).

[0054] (b) The triethoxyphosphorus solution of 2,7-dibromo-9,9-di(3-bromopropyl)fluorene was heated to 140°C and refluxed for 16 hours. After the reaction was completed, the solution was cooled and the excess triethoxyphosphorus was evaporated under reduced pressure. The residual material was separated using a neutral alumina column, and impurities were removed using an eluent of ethyl acetate / petroleum ether = 1:1. Ethyl acetate was then used as the eluent to obtain white granular microcrystals (2,7-dibromo-9,9-di(3-phosphoethylpropyl)fluorene).

[0055] (c) 2,7-Dibromo-9,9-bis(3-phosphoethylpropyl)fluorene was dissolved in dichloromethane, and trimethylsilyl bromide was added dropwise under argon protection. After the addition was complete, the reaction was carried out at room temperature for 10 hours. After the reaction was completed, the excess trimethylsilyl bromide and dichloromethane were removed under reduced pressure. The residual material was dissolved in methanol. After stirring at room temperature for 6 hours, the methanol was removed under reduced pressure again to obtain a light yellow solid. The solid was ultrasonically washed with water until white and then dried in vacuo at 50°C for 12 hours to obtain a white powdery solid (2,7-dibromo-9,9-bis(3-phosphopropyl)fluorene).

[0056] (d) Under argon protection, 2,7-dibromo-9,9-di(3-phosphopropyl)fluorene, 1,4-phenylenediboronic acid bis(pinacol) ester, Pd(dppf)Cl 2 , N,N-dimethylformamide and 2M Na 2 CO 3 Aqueous solution, under argon protection, stirred and reacted at 85°C for 60 hours, phenylboric acid was dissolved in N,N-dimethylformamide, the air was exhausted for 30 minutes after ventilation, and the reaction was introduced into a reaction bottle for 5 hours. Bromobenzene was added to the reaction bottle and reacted for another 5 hours. After the reaction was completed, the reaction solution was injected into cold acetone, and the precipitated solid was filtered and vacuum dried and then dissolved in distilled water again. The solution was dialyzed through a dialysis membrane for 3 days, and the water was changed every 6 hours. After the dialysis was completed, the solution in the dialysis membrane was concentrated and precipitated in acetone again. After filtration and vacuum drying, a dark yellow powdery solid was obtained, namely polyfluorene.

[0057] The following examples all use the polyfluorene prepared as described above.

[0058] Example 1

[0059] The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane comprises the following steps:

[0060] (1) Preparation of polyfluorene-copper oxide:

[0061] a. Dissolve 1.7 g of polyfluorene in 40 mL of water to obtain a polyfluorene solution.

[0062] b. 2.14 gCu(CH 3 COO 2 ·H 2 O was dissolved in 40 mL of distilled water, and then the polyfluorene solution was added.

[0063] c. Continue to slowly drip in 2.3 mL of ammonia water, stir for 30 min, then add NaOH to maintain the pH at 11, stir for 30 min to obtain a homogeneous solution.

[0064] d. The homogeneous solution was subjected to hydrothermal reaction at 180°C for 32 h, and washed with distilled water and ethanol to obtain a black precipitate.

[0065] e. Dry the black precipitate in an oven at 50°C for 16 h to obtain polyfluorene-copper oxide.

[0066] (2) Dissolve 20 g PVA1799 in 180 mL water and stir at 85 °C for 2 h to obtain a PVA solution;

[0067] (3) Add 4 g of polyfluorene-copper oxide to the PVA solution and stir at 70 °C for 2 h to obtain a PVA / polyfluorene-copper oxide solution.

[0068] (4) Add 3 g of citric acid (CA) to the PVA / polyfluorene-copper oxide solution and stir the mixture at room temperature for 1.5 h to obtain a PVA-CA / polyfluorene-copper oxide solution.

[0069] (5) The PVA-CA / polyfluorene-copper oxide solution was transferred to a 10 mL syringe with a voltage-regulated DC power supply, with the tip 16 cm away from the collector. The solution was pumped at a steady flow rate of 0.24 mL / h and an applied voltage of 15 kV for 2 h using electrospinning, and then collected to obtain the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane.

[0070] Example 2

[0071] The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane comprises the following steps:

[0072] (1) Preparation of polyfluorene-copper oxide:

[0073] a. Dissolve 1.7 g of polyfluorene in 40 mL of water to obtain a polyfluorene solution.

[0074] b. Add 2.14 g of Cu(CH 3 COO 2 ·H 2 O was dissolved in 40 mL of distilled water, and then the polyfluorene solution was added.

[0075] c. Continue to slowly drip in 2.3 mL of ammonia water, stir for 40 min, then add KOH to maintain the pH at 10.5, stir for 50 min to obtain a homogeneous solution.

[0076] d. The homogeneous solution was subjected to hydrothermal reaction at 200°C for 24 h, and washed with distilled water and ethanol to obtain a black precipitate.

[0077] e. Dry the black precipitate in an oven at 60°C for 12 h to obtain polyfluorene-copper oxide.

[0078] (2) Dissolve 24 g PVA1799 in 216 mL water and stir at 80 °C for 2 h to obtain a PVA solution;

[0079] (3) Add 4 g of polyfluorene-copper oxide to the PVA solution and stir at 80 °C for 1.5 h to obtain a PVA / polyfluorene-copper oxide solution.

[0080] (4) Add 4.8 g of citric acid (CA) to the PVA / polyfluorene-copper oxide solution and stir the mixture at room temperature for 2 h to obtain a PVA-CA / polyfluorene-copper oxide solution.

[0081] (5) The PVA-CA / polyfluorene-copper oxide solution was transferred to a 10 mL syringe with a voltage-regulated DC power supply, with the tip 17 cm away from the collector. The solution was pumped at a steady flow rate of 0.26 mL / h and an applied voltage of 14.5 kV for 1.5 h using electrospinning, and then collected to obtain the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane.

[0082] Example 3

[0083] The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane comprises the following steps:

[0084] (1) Preparation of polyfluorene-copper oxide:

[0085] a. Dissolve 1.7 g of polyfluorene in 40 mL of water to obtain a polyfluorene solution.

[0086] b. 1.92 g of Cu(CH 3 COO 2 ·H 2 O was dissolved in 35.9 mL of distilled water, and then the polyfluorene solution was added.

[0087] c. Continue to slowly drip 1.8 mL of ammonia water, stir for 35 min, then add NaOH to maintain the pH at 11, stir for 60 min to obtain a homogeneous solution.

[0088] d. The homogeneous solution was subjected to hydrothermal reaction at 190°C for 26 h, and washed with distilled water and ethanol to obtain a black precipitate.

[0089] e. Dry the black precipitate in an oven at 55°C for 12 h to obtain polyfluorene-copper oxide.

[0090] (2) Dissolve 22 g of PVA1799 in 198 mL of water and stir at 90 °C for 1.5 h to obtain a PVA solution;

[0091] (3) Add 4 g of polyfluorene-copper oxide to the PVA solution and stir at 75 °C for 2 h to obtain a PVA / polyfluorene-copper oxide solution.

[0092] (4) Add 4 g of citric acid (CA) to the PVA / polyfluorene-copper oxide solution and stir the mixture at room temperature for 2 h to obtain a PVA-CA / polyfluorene-copper oxide solution.

[0093] (5) The PVA-CA / polyfluorene-copper oxide solution was transferred to a 10 mL syringe with a voltage-regulated DC power supply, with the tip 16 cm away from the collector. The solution was pumped at a steady flow rate of 0.24 mL / h and an applied voltage of 15 kV for 2 h using electrospinning, and then collected to obtain the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane.

[0094] Example 4

[0095] The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane comprises the following steps:

[0096] (1) Preparation of polyfluorene-copper oxide:

[0097] a. Dissolve 1.7 g of polyfluorene in 40 mL of water to obtain a polyfluorene solution.

[0098] b. Add 2.00 g of Cu(CH 3 COO 2 ·H 2 O was dissolved in 37.4 mL of distilled water, and then the polyfluorene solution was added.

[0099] c. Continue to slowly drip in 2 mL of ammonia water, stir for 35 min, then add NaOH to maintain the pH at 11, stir for 40 min to obtain a homogeneous solution.

[0100] d. The homogeneous solution was subjected to hydrothermal reaction at 180°C for 24 h, and washed with distilled water and ethanol to obtain a black precipitate.

[0101] e. Dry the black precipitate in an oven at 50°C for 12 h to obtain polyfluorene-copper oxide.

[0102] (2) Dissolve 20 g PVA1799 in 180 mL water and stir at 85 °C for 2 h to obtain a PVA solution;

[0103] (3) Add 4 g of polyfluorene-copper oxide to the PVA solution and stir at 75 °C for 2 h to obtain a PVA / polyfluorene-copper oxide solution.

[0104] (4) Add 3 g of citric acid (CA) to the PVA / polyfluorene-copper oxide solution and stir the mixture at room temperature for 2 h to obtain a PVA-CA / polyfluorene-copper oxide solution.

[0105] (5) The PVA-CA / polyfluorene-copper oxide solution was transferred to a 10 mL syringe with a voltage-regulated DC power supply, with the tip 16 cm away from the collector. The solution was pumped at a steady flow rate of 0.24 mL / h and an applied voltage of 15 kV for 2 h using electrospinning, and then collected to obtain the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane.

[0106] Comparative Example 1

[0107] A method for preparing a PVA-CA fiber membrane comprises the following steps:

[0108] (1) Dissolve 20 g PVA1799 in 180 mL water and stir at 85 °C for 2 h to obtain a PVA solution;

[0109] (2) Add 3 g of citric acid (CA) and stir the mixture at room temperature for 1.5 h to obtain a PVA-CA solution.

[0110] (3) The PVA-CA solution was transferred into a 10 mL syringe with a voltage-regulated DC power supply, with the tip 16 cm away from the collector. The solution was pumped at a steady flow rate of 0.24 mL / h and an applied voltage of 15 kV for 2 h using electrospinning to form a membrane, and then collected to obtain the PVA-CA fiber membrane.

[0111] Comparative Example 2

[0112] A method for preparing a PVA-CA / polyfluorene fiber composite film comprises the following steps:

[0113] (1) 1.7 g of the same polyfluorene as in Example 1 was dissolved in 40 mL of water to obtain a polyfluorene solution.

[0114] (2) Dissolve 20 g PVA1799 in 180 mL water and stir at 85 °C for 2 h to obtain a PVA solution;

[0115] (3) Add the polyfluorene solution to the PVA solution and stir at 70 °C for 2 h to obtain a PVA / polyfluorene solution.

[0116] (4) Add 3 g of citric acid (CA) to the PVA / polyfluorene solution and stir the mixture at room temperature for 1.5 h to obtain a PVA-CA / polyfluorene solution.

[0117] (5) The PVA-CA / polyfluorene solution was transferred into a 10 mL syringe with a voltage-regulated DC power supply, with the tip 16 cm away from the collector. The solution was pumped at a steady flow rate of 0.24 mL / h and an applied voltage of 15 kV for 2 h using electrospinning, and then collected to obtain the PVA-CA / polyfluorene fiber composite membrane.

[0118] Comparative Example 3

[0119] A method for preparing a PVA-CA / copper oxide nanofiber composite membrane comprises the following steps:

[0120] (1) 2.14 g Cu(CH 3 COO 2 ·H 2O was dissolved in 40 mL of distilled water, and 2.3 mL of ammonia water was slowly added, stirred for 30 min, and NaOH was added to maintain the pH at 11, stirred for 30 min to obtain a homogeneous solution, and the homogeneous solution was subjected to hydrothermal reaction at 180 ° C for 32 h, washed with distilled water and ethanol to obtain a precipitate, and the precipitate was dried in an oven at 50 ° C for 16 h to obtain copper oxide.

[0121] (2) Dissolve 20 g PVA1799 in 180 mL water and stir at 85 °C for 2 h to obtain a PVA solution;

[0122] (3) Add 4 g of copper oxide to the PVA solution and stir at 70 °C for 2 h to obtain a PVA / copper oxide solution.

[0123] (4) Add 3 g of citric acid (CA) to the PVA / copper oxide solution and stir the mixture at room temperature for 1.5 h to obtain a PVA-CA / copper oxide solution.

[0124] (5) The PVA-CA / copper oxide solution was transferred to a 10 mL syringe with a voltage-regulated DC power supply, with the tip 16 cm away from the collector. The solution was pumped at a steady flow rate of 0.24 mL / h and an applied voltage of 15 kV for 2 h using electrospinning, and then collected to obtain the PVA-CA / copper oxide nanofiber composite membrane.

[0125] Comparative Example 4

[0126] A method for preparing a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane comprises the following steps:

[0127] (1) Preparation of polyfluorene-copper oxide:

[0128] a. Dissolve 1.7 g of polyfluorene in 40 mL of water to obtain a polyfluorene solution.

[0129] b. 2.14 gCu(CH 3 COO 2 ·H 2 O was dissolved in 40 mL of distilled water, and then the polyfluorene solution was added.

[0130] c. Continue to slowly drip NaOH to maintain the pH at 11 and stir for 30 minutes to obtain a homogeneous solution.

[0131] d. The homogeneous solution was subjected to hydrothermal reaction at 180°C for 32 h, and washed with distilled water and ethanol to obtain a black precipitate.

[0132] e. Dry the black precipitate in an oven at 50°C for 16 h to obtain polyfluorene-copper oxide.

[0133] (2) Dissolve 20 g PVA1799 in 180 mL water and stir at 85 °C for 2 h to obtain a PVA solution;

[0134] (3) Add 4 g of polyfluorene-copper oxide to the PVA solution and stir at 70 °C for 2 h to obtain a PVA / polyfluorene-copper oxide solution.

[0135] (4) Add 3 g of citric acid (CA) to the PVA / polyfluorene-copper oxide solution and stir the mixture at room temperature for 1.5 h to obtain a PVA-CA / polyfluorene-copper oxide solution.

[0136] (5) The PVA-CA / polyfluorene-copper oxide solution was transferred to a 10 mL syringe with a voltage-regulated DC power supply, with the tip 16 cm away from the collector. The solution was pumped at a steady flow rate of 0.24 mL / h and an applied voltage of 15 kV for 2 h using electrospinning, and then collected to obtain the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane.

[0137] The fiber membranes prepared in the above examples and comparative examples were tested for the following properties, and the test results are shown in Table 1.

[0138] 1. Ethylene catalytic effect test:

[0139] In the photoreactor, ethylene photocatalysis reaction is carried out by irradiation with a xenon lamp.

[0140] First, various nanofibers to be tested were placed in a photoreactor. 100 μL of ethylene was injected into the photoreactor, and a fan was used to circulate the gas evenly. The initial concentration of ethylene was measured using gas chromatography until steady-state conditions were reached in the photoreactor. Then the xenon lamp was turned on to continuously irradiate the nanofibers in the reactor for 6 h, and samples were taken every 1 h to measure the concentration of ethylene in the reactor. The ethylene degradation rate of various nanofibers to be tested was calculated according to the equation.

[0141] 2. Sterilization effect test:

[0142] Single colonies of Escherichia coli and Staphylococcus aureus were inoculated in Luria-Bertani medium and incubated at 37°C for 24 h. The surface was coated with different concentrations of nanocomposites, immersed in the bacterial suspension under the irradiation of a xenon lamp, and incubated with the bacterial suspension at 37°C with shaking for 12 h. Finally, the bacterial suspension was spread on an agar plate and incubated in an incubator at 37°C for 20 h. The colonies were observed in the agar plate and counted using an automatic colony counter.

[0143] Tensile properties: tested according to GB / T1040 standard

[0144] Degradation performance: tested according to the standard of GB / T19277.1-2011.

[0145] Table 1 Test results

[0146]

[0147] From the above, it can be seen that the product prepared by the present invention is not only a degradable film material, but also has the ability of antibacterial and ethylene removal, which fundamentally solves the problem of preservation. The product prepared by the present invention has excellent preservation ability and is a functional and environmentally friendly packaging material.

Claims

1. A method for preparing a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane, characterized in that: The following steps are involved: (1) Dissolve PVA in water and stir at 80-90°C for 1.5-2h to obtain a PVA solution; (2) adding polyfluorene-copper oxide to the PVA solution and stirring at 70-80° C. for 1.5-2 h to obtain a PVA / polyfluorene-copper oxide solution; (3) Add citric acid to the PVA / polyfluorene-copper oxide solution and react at room temperature for 1.5-2 hours to obtain a PVA-CA / polyfluorene-copper oxide solution; (4) preparing a PVA-CA / polyfluorene-copper oxide nanofiber composite membrane by electrospinning the PVA-CA / polyfluorene-copper oxide solution; The preparation method of polyfluorene-copper oxide comprises the following steps: a. dissolving polyfluorene in water to obtain a polyfluorene solution; b. Dissolve copper acetate in distilled water and then add polyfluorene solution; c. Continue to drip ammonia water, stir for 30-40 minutes, then add alkali to maintain the pH at 10.5-11, stir for 30-60 minutes to obtain a homogeneous solution; d. subjecting the homogeneous solution to a hydrothermal reaction at 180-200° C. for 24-32 hours, and washing to obtain a black precipitate; e. Dry the black precipitate at 50-60° C. for 12-16 h to obtain polyfluorene-copper oxide; The preparation method of the polyfluorene comprises the following steps: (a) A mixture of 2,7-dibromofluorene, tetrabutylammonium bromide, 1,3-dibromopropane and sodium hydroxide aqueous solution is heated to 70°C, refluxed for 8 hours, cooled to room temperature, extracted with dichloromethane, the organic phase is washed three times with distilled water, washed once with saturated brine, dried with Na2SO4, dichloromethane is removed, and excess 1,3-dibromopropane is removed under reduced pressure. The residual material is separated by column to obtain a white powdery solid, which is triethoxyphosphorus of 2,7-dibromo-9,9-di(3-bromopropyl)fluorene; (b) The triethoxyphosphorus solution of 2,7-dibromo-9,9-di(3-bromopropyl)fluorene was heated to 140°C and refluxed for 16 hours. After the reaction was completed, the solution was cooled and the excess triethoxyphosphorus was distilled off under reduced pressure. The residual material was separated by a neutral alumina column, and impurities were removed by using an ethyl acetate / petroleum ether = 1:1 eluent. Then, ethyl acetate was used as the eluent to obtain white granular microcrystals, which were 2,7-dibromo-9,9-di(3-phosphoethyl ester propyl)fluorene. (c) 2,7-dibromo-9,9-bis(3-phosphoethylpropyl)fluorene was dissolved in dichloromethane, trimethylsilyl bromide was added dropwise under argon protection, and the reaction was carried out at room temperature for 10 hours. After the reaction was completed, the excess trimethylsilyl bromide and dichloromethane were removed under reduced pressure, and the residual material was dissolved in methanol. After stirring at room temperature for 6 hours, the methanol was removed under reduced pressure again to obtain a light yellow solid. The solid was ultrasonically washed with water until white, and then vacuum dried at 50°C for 12 hours to obtain a white powder solid. The white powder solid is 2,7-dibromo-9,9-bis(3-phosphopropyl)fluorene; (d) Under argon protection, 2,7-dibromo-9,9-di(3-phosphopropyl)fluorene, 1,4-phenylenediboronic acid bis(pinacol) ester, Pd(dppf)Cl2, N,N-dimethylformamide and 2M Na2CO3 aqueous solution were added to a reaction bottle connected to a double-row tube. The reaction was stirred at 85°C for 60 hours under argon protection. Phenylboric acid was dissolved in N,N-dimethylformamide, and the air was exhausted for 30 minutes after ventilation. The mixture was introduced into the reaction bottle and reacted for 5 hours. Bromobenzene was added to the reaction bottle and reacted for another 5 hours. After the reaction was completed, the reaction solution was injected into cold acetone. The precipitated solid was filtered and vacuum dried, then dissolved in distilled water again. The solution was dialyzed through a dialysis membrane for 3 days, with the water changed every 6 hours. After the dialysis was completed, the solution in the dialysis membrane was concentrated and precipitated in acetone again. After filtration and vacuum drying, a dark yellow powdery solid was obtained, namely polyfluorene.

2. The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane according to claim 1, characterized in that: The mass ratio of PVA to polyfluorene-copper oxide is (5:1)-(6:1).

3. The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane according to claim 1, characterized in that: The mass ratio of PVA to citric acid is (20:3)-(5:1).

4. The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane according to claim 1, characterized in that: The process parameters of the electrospinning in step (4) are: a stable flow rate of 0.24-0.26 mL / h, an applied voltage of 14.5-15 kV, and a pumping time of 1.5-2 h; the electrospinning uses a syringe with a DC power supply regulation, and the tip is 16-17 cm away from the collector.

5. The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane according to claim 1, characterized in that: The molar ratio of copper acetate to ammonia water is 1:(1.2-1.5).

6. The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane according to claim 1, characterized in that: The mass ratio of polyfluorene to copper acetate is 1:(1.13-1.26).

7. The method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane according to claim 1, characterized in that: The base is NaOH or KOH.

8. A PVA-CA / polyfluorene-copper oxide nanofiber composite membrane, characterized in that: The composite membrane is prepared by the method for preparing the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane described in any one of claims 1 to 7.

9. An application of the PVA-CA / polyfluorene-copper oxide nanofiber composite membrane according to claim 8, characterized in that: Used for preservation of fruits and vegetables.