A Mg2P2O7 / nitrogen-doped biomass carbon composite catalyst and its preparation method and application

By preparing Mg2P2O7/nitrogen doped biomass carbon composite catalyst, the problem of low degradation efficiency of activated PMS by single biomass carbon is solved, and efficient degradation of organic pollutants such as tetracycline and multiple cycles is achieved. It is suitable for water bodies Purification.

CN118681587BActive Publication Date: 2024-12-06CHINA UNIV OF MINING & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410893938.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-12-06
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The inefficiency of single biomass charcoal to catalyze the degradation of organic pollutants by activation of permonosulfate (PMS), limiting its application potential in water purification.

Method used

Using Mg2P2O7/nitrogen doped biomass carbon composite catalyst, the biomass is prepared by grinding and mixing it with one step of calcining, forming an irregular sheet-like structure rich in pores, which is used to activate PMS to improve its degradation of tetracycline, etc. Performance of organic pollutants.

Benefits of technology

The performance of PMS degrading organic pollutants such as tetracycline is significantly improved, and the rapid degradation of a variety of organic pollutants is achieved. The catalyst maintains high efficiency and activity in multiple cycles, making it suitable for industrial wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118681587B_ABST
    Figure CN118681587B_ABST
Patent Text Reader

Abstract

The invention discloses a Mg2P2O7 / nitrogen-doped biochar composite catalyst and a preparation method and application thereof, and belongs to the technical field of sewage treatment. The fallen leaves of Chinese parasol trees are washed and dried, ground and mixed with magnesium ammonium phosphate hexahydrate, and then calcined in one step to obtain the Mg2P2O7 / nitrogen-doped biochar composite catalyst. The preparation method provided by the invention has a simple process and is easy to operate. The Mg2P2O7 / nitrogen-doped biochar composite catalyst with high efficiency and activity of the invention has high catalytic activity and fast degradation rate for various pollutants. It can be used to activate persulfate and efficiently degrade organic pollutants in water bodies, and can achieve rapid degradation of organic pollutants in complex actual water bodies, and has good application prospects in industrial wastewater and practical applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sewage treatment, and in particular relates to a Mg2P2O7 / nitrogen-doped biomass charcoal composite catalyst and a preparation method and application thereof. Background Art

[0002] Tetracycline is a broad-spectrum antibiotic widely used in clinical medicine. Compared with traditional treatment methods, advanced oxidation methods have the characteristics of strong oxidation ability, high reaction rate and no secondary pollution. Advanced oxidation technology based on permonosulfate (PMS) is considered to be a promising technology for treating organic pollutants. Since PMS activation can produce sulfate radicals with strong oxidation ability, it has broad application prospects.

[0003] PMS can be activated by ultraviolet, heat, ultrasound, transition metals and carbon materials. Among them, carbon materials are the most commonly used PMS activators. However, pure carbon materials generally have poor catalytic reaction activity, which greatly limits their application potential. By doping them with nitrogen atoms or loading metal / metal compounds on their surface, the electron density of carbon atoms can be adjusted or the synergistic effect between metal / metal compounds and carbon materials can be enhanced, thereby improving their catalytic activity.

[0004] Converting solid waste into catalysts to treat tetracycline in water is of great significance to environmental treatment. As a common waste, dead leaves can be calcined to obtain biomass carbon materials; solid waste (struvite) generated when treating high-ammonia nitrogen wastewater is rich in nitrogen and metal elements, which helps to improve the catalytic performance of carbon materials.

[0005] Therefore, it is considered to prepare the two wastes, struvite and dead leaves, into activated PMS catalysts for oxidative degradation of organic pollutants through calcination, which can achieve water purification while removing solid waste, which has dual significance for environmental treatment. Summary of the invention

[0006] In view of the problem that single biochar is inefficient in activating PMS to catalyze the degradation of organic pollutants, the present invention provides a Mg2P2O7 / nitrogen-doped biochar composite catalyst and a preparation method and application thereof. The prepared composite catalyst has high performance in activating PMS to degrade tetracycline.

[0007] The present invention is achieved through the following technical solutions:

[0008] A Mg2P2O7 / nitrogen-doped biomass carbon composite catalyst, wherein the composite catalyst has an irregular flaky structure morphology rich in holes.

[0009] A method for preparing the composite catalyst is to grind and mix biomass with magnesium ammonium phosphate hexahydrate and then calcine in one step to obtain a Mg2P2O7 / nitrogen-doped biomass carbon composite catalyst.

[0010] Furthermore, the biomass is frozen fallen leaves; and the fallen leaves are sycamore leaves.

[0011] Furthermore, the mass ratio of the biomass to magnesium ammonium phosphate hexahydrate is 4:1-8.

[0012] Furthermore, the calcination temperature is 500-1000 °C, and the heating rate is 2-8 °C min −1 ; The calcination atmosphere is a mixed atmosphere of argon and hydrogen.

[0013] Furthermore, the freeze-dried dead leaves were uniformly mixed with magnesium ammonium phosphate hexahydrate and calcined, then washed with 0.5 M sulfuric acid and deionized water for more than three times, and dried in a vacuum drying oven at 80 °C for 12 h.

[0014] An application of the above-mentioned Mg2P2O7 / nitrogen-doped biochar composite catalyst in degrading organic pollutants in wastewater.

[0015] Furthermore, the above application adopts the following method: mixing the Mg2P2O7 / nitrogen-doped biochar composite catalyst with organic pollutant wastewater, and adding persulfate to react.

[0016] Furthermore, the addition amount of the Mg2P2O7 / nitrogen-doped biochar composite catalyst is 0.05 g to 0.15 g per liter of organic pollutant wastewater; the addition amount of the persulfate is 0.5 mM to 0.8 mM per liter of organic pollutant wastewater; and the initial concentration of organic pollutants in the organic pollutant wastewater is 10 mg / L to 30 mg / L.

[0017] Furthermore, the persulfate is peroxymonosulfate; the organic pollutants in the organic pollutants are one or more of tetracycline, oxytetracycline, rhodamine B, methylene blue, methyl orange and orange II; and the degradation time is 30 minutes.

[0018] Beneficial Effects

[0019] The Mg2P2O7 / nitrogen-doped biochar composite catalyst prepared by the present invention has a simple preparation method and is easy to operate; the Mg2P2O7 / nitrogen-doped biochar composite catalyst has a high catalytic activity, and has a good degradation effect on various organic pollutants such as tetracycline, oxytetracycline, rhodamine B, methylene blue, methyl orange, orange yellow II, etc., and can be used to activate persulfate and efficiently degrade organic pollutants in water bodies, and can achieve rapid degradation of organic pollutants in complex actual water bodies, and has a good application prospect in industrial wastewater and practical applications. Moreover, the Mg2P2O7 / nitrogen-doped biochar composite catalyst prepared by the present invention is recycled for multiple rounds, and the catalytic activity remains unchanged after re-calcination, and can be recycled for multiple times. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a scanning electron microscope image of the Mg2P2O7 / nitrogen-doped biomass carbon composite catalyst prepared in Example 3;

[0021] Figure 2 (a) Transmission electron microscopy image, (b) high-resolution transmission electron microscopy image, (c) high-angle annular dark field scanning transmission, and (d) C, (e) N, (f) P, (g) O, and (h) Mg element mapping images of the Mg2P2O7 / nitrogen-doped biochar composite catalyst prepared in Example 3;

[0022] Figure 3 X-ray photoelectron spectra of the Mg2P2O7 / nitrogen-doped biochar composite catalyst in Example 3, wherein (a) is the full spectrum, (b) C 1s, (c) N 1s, (d) P 2p, (e) O 1s, and (f) Mg 1s high-resolution X-ray photoelectron spectra;

[0023] Figure 4 The degradation performance diagram of tetracycline by the Mg2P2O7 / nitrogen-doped biomass charcoal composite catalyst prepared in Examples 1-5 and the materials prepared in Comparative Examples 1-3;

[0024] Figure 5 The degradation performance diagram of tetracycline by the Mg2P2O7 / nitrogen-doped biomass char composite catalyst prepared in Example 3 and Examples 6-10;

[0025] Figure 6 This is a graph showing the multi-cycle stability test of the Mg2P2O7 / nitrogen-doped biochar composite catalyst in the tetracycline degradation process in Example 3;

[0026] Figure 7 This is a graph showing the degradation performance of the Mg2P2O7 / nitrogen-doped biochar composite catalyst prepared in Example 3 for oxytetracycline, rhodamine B, methylene blue, methyl orange, and orange II. DETAILED DESCRIPTION

[0027] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0028] Example 1

[0029] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 4:1). The ground and mixed powder was then calcined at 900 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 1−900.

[0030] Example 2

[0031] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 2:1). The ground and mixed powder was then calcined at 900 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 2−900.

[0032] Example 3

[0033] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 1:1). The ground and mixed powder was then calcined at 900 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 3−900.

[0034] Example 4

[0035] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 2:3). The ground and mixed powder was then calcined at 900 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 4−900.

[0036] Example 5

[0037] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 1:2). The ground and mixed powder was then calcined at 900 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 5−900.

[0038] Example 6

[0039] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 1:1). The ground and mixed powder was then calcined at 500 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 3−500.

[0040] Example 7

[0041] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 1:1). The ground and mixed powder was then calcined at 600 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 3−600.

[0042] Example 8

[0043] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 1:1). The ground and mixed powder was then calcined at 700 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 3−700.

[0044] Example 9

[0045] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 1:1). The ground and mixed powder was then calcined at 800 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried under vacuum at 80 °C for 12 h. The obtained material was MBC / 3−800.

[0046] Example 10

[0047] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ball-milled and mixed with magnesium ammonium phosphate hexahydrate (mass ratio 1:1). The ground and mixed powder was then calcined at 1000 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected, washed with 0.5 M sulfuric acid, and then washed three times with deionized water, and dried in vacuum at 80 °C for 12 h. The obtained material was MBC / 3−1000.

[0048] Comparative Example 1

[0049] The collected dead leaves were cleaned and freeze-dried, and the freeze-dried dead leaves were ground in a ball mill. The ground dead leaves were placed in a porcelain boat and calcined in a tube furnace at 900 °C for 2 h in a mixed atmosphere of argon and hydrogen, with a heating rate of 5 °C min −1 The calcined powder was collected and washed with 0.5 M sulfuric acid and then washed three times with deionized water, and finally dried in a vacuum oven at 80 °C for 12 h. The obtained material is biochar.

[0050] Comparative Example 2

[0051] Magnesium ammonium phosphate hexahydrate was placed in a porcelain boat and calcined at 900 °C for 2 h in a mixed atmosphere of argon and hydrogen using a tube furnace with a heating rate of 5 °C min −1 The calcined powder was collected, washed three times with deionized water, and finally dried in a vacuum oven at 80 °C for 12 h. The obtained material was Mg2P2O7.

[0052] Comparative Example 3

[0053] 40 mg of PMS was added to 100 mL of tetracycline solution (20 mg L -1 ) triggered the reaction and effectively degraded 18% of tetracycline within 30 min.

[0054] Performance Test:

[0055] The scanning electron microscope image of the Mg2P2O7 / nitrogen-doped biomass carbon composite catalyst (MBC / 3-900) prepared in Example 3 is as follows: Figure 1 As shown, it can be seen that the Mg2P2O7 / nitrogen-doped biochar composite catalyst (MBC / 3-900) prepared in Example 3 has an irregular flaky structure morphology rich in holes; the transmission electron microscopy image, high-resolution transmission electron microscopy image, high-angle annular dark field scanning transmission and element mapping image of the Mg2P2O7 / nitrogen-doped biochar composite catalyst (MBC / 3-900) prepared in Example 3 are shown in FIG. Figure 2 As shown, (a) is a transmission electron microscope image, (b) is a high-resolution transmission electron microscope image, (c) is a high-angle annular dark field scanning transmission image, and (d) C, (e) N, (f) P, (g) O and (h) Mg element mapping images; Figure 2 a It can be seen that the Mg2P2O7 / nitrogen-doped biochar composite catalyst (MBC / 3-900) presents an obvious flaky structure, and obvious particles can be seen on the surface. Figure 2 In the high-resolution transmission electron microscope image shown in b, the crystal plane with a lattice spacing of 0.349 nm corresponds to the (021) of Mg2P2O7, and the crystal plane with a lattice spacing of 0.34 nm corresponds to the (002) of C. Figure 2 c is a high-angle annular dark field scanning transmission image and Figure 2 From the element mapping diagram of d-2h, it can be seen that the five elements C, N, O, P and Mg are evenly distributed in MBC / 3-900.

[0056] The XPS graph of the Mg2P2O7 / nitrogen-doped biochar composite catalyst (MBC / 3-900) in Example 3 is as follows: Figure 3 As shown, (a) is the full spectrum of X-ray photoelectron spectrum, (b) C1s, (c) N 1s, (d) P 2p, (e) O 1s, (f) Mg 1s high-resolution X-ray photoelectron spectrum; Figure 3 It can be seen that MBC / 3-900 is mainly composed of four elements: C, N, O and P. Figure 3 As shown in b, the C1s spectrum contains sp 2 The peaks of C, CN, CO and C=O confirm that biochar contains a variety of active functional groups. Figure 3 c shows that the three peaks in the N 1s spectrum correspond to pyridinic N, pyridinic N, and graphitic N, respectively. Figure 3 In e, CO and C=O signals appear in the O element binding energy region, and the remaining PO, POP and Mg-O are all attributed to Mg2P2O7. Figure 3 d and Figure 3 f The peaks appearing in the P 2p and Mg 1s spectra respectively correspond to standard Mg2P2O7.

[0057] The degradation performance of the Mg2P2O7 / nitrogen-doped biomass carbon composite catalyst prepared in Example 1-5 for tetracycline is shown in the figure Figure 4 shown by Figure 4 It can be seen that the degradation ability of comparative example 1 (biochar) and comparative example 2 (Mg2P2O7) on tetracycline is very weak, with a degradation of 25% in 30 minutes; the degradation ability of comparative example 3 (only PMS) on tetracycline is even weaker, with a degradation of 18% in 30 minutes; while the Mg2P2O7 / nitrogen-doped biochar composite catalyst has a stronger degradation ability, and the maximum degradation of the composite material in Examples 2-4 is 85% in 30 minutes.

[0058] The degradation performance of Mg2P2O7 / nitrogen-doped biomass carbon composite catalysts prepared in Example 3 and Examples 6-10 for tetracycline is shown in the figure Figure 5 shown by Figure 5 It can be seen that the composite catalysts prepared in Examples 6 and 7 have a slower degradation rate and a lower removal rate for tetracycline, while the composite catalysts prepared in Examples 3 and 8-10 have a faster degradation rate and a higher removal rate for tetracycline. Among them, the composite catalyst prepared in Example 3 has the fastest degradation rate and the highest removal rate for tetracycline. Figure 6 As shown by Figure 6 It can be seen that the removal rate of tetracycline gradually decreased in the same period of time for the Mg2P2O7 / nitrogen-doped biomass carbon composite catalyst prepared in Example 3. After the used MBC / 3-900 was annealed and retested, the catalytic performance of MBC / 3-900 returned to the initial state.

[0059] The degradation performance of the Mg2P2O7 / nitrogen-doped biochar composite catalyst prepared in Example 3 on oxytetracycline, rhodamine B, methylene blue, methyl orange, and orange II is as follows: Figure 7 shown by Figure 7It can be seen that the degradation rates of the composite catalyst prepared in Example 3 for oxytetracycline, rhodamine B, methylene blue, methyl orange, and orange II are all higher than 80%. According to literature reports, PMS degrades oxytetracycline by 16.6% in 30 minutes (Chemical Engineering Journal, 2022, 436, 135199); PMS degrades rhodamine B by 23.4% in 25 minutes (Journal of Southwest University (Natural Science Edition), 2024, 46(7): 127-136); PMS degrades methylene blue by 9.32% in 50 minutes (Journal of Inorganic Chemistry, 2022, 38(11): 2192-2201); PMS degrades methyl orange by 30% in 20 minutes (Environmental Science Research, 2018, 31(1): 123-129); PMS degrades orange II by 11% in 30 minutes (Journal of Environmental Engineering, 2021, 15(7): 2274-2286). That is, the degradation rates of PMS for oxytetracycline, rhodamine B, methylene blue, methyl orange, and orange II are relatively low. The degradation effect of the composite catalyst prepared in Example 3 is significantly improved.

Claims

1. A Mg2P2O7 / nitrogen-doped biochar composite catalyst, characterized in that: The composite catalyst has an irregular sheet structure rich in holes. The preparation method of the composite catalyst comprises: grinding and mixing freeze-dried dead leaves with magnesium ammonium phosphate hexahydrate by ball milling, and then calcining in one step to obtain a Mg2P2O7 / nitrogen-doped biomass carbon composite catalyst; the mass ratio of the freeze-dried dead leaves to magnesium ammonium phosphate hexahydrate is 4:1-8; the calcination temperature is 500-1000°C, and the heating rate is 5°C min -1 The calcination atmosphere is a mixed atmosphere of argon and hydrogen; the freeze-dried dead leaves are evenly mixed with magnesium ammonium phosphate hexahydrate and calcined, then washed with 0.5 M sulfuric acid and deionized water for more than three times, and dried in a vacuum drying oven at 80°C for 12h.

2. Use of the Mg2P2O7 / nitrogen-doped biochar composite catalyst according to claim 1 in degrading organic pollutants in wastewater.

3. The use according to claim 2, characterized in that: The following method is adopted: Mg2P2O7 / nitrogen-doped biochar composite catalyst is mixed with organic pollutant wastewater, and persulfate is added for reaction.

4. The use according to claim 3, characterized in that: The addition amount of the Mg2P2O7 / nitrogen-doped biochar composite catalyst is 0.05 g to 0.15 g per liter of organic pollutant wastewater; the addition amount of the persulfate is 0.5 mM to 0.8 mM per liter of organic pollutant wastewater; the initial concentration of organic pollutants in the organic pollutant wastewater is 10 mg / L to 30 mg / L.

5. The use according to claim 3, characterized in that: The persulfate is peroxymonosulfate; the organic pollutants in the organic pollutant wastewater are one or more of tetracycline, oxytetracycline, rhodamine B, methylene blue, methyl orange and orange II; and the degradation time is 30 minutes.

Citation Information

Patent Citations

  • Method of utilizing phosphated residue to prepare dye photodegradation catalyst

    CN105772043A

  • Method for degrading organic pollutants in wastewater by catalyzing persulfate

    CN107298477A

  • Method for degrading organic pollutants in water body by activating persulfate with magnetic nitrogen-doped carbon

    CN112374601A

  • Preparation method of supported modified activated carbon ozone catalyst

    CN114917908A

  • Preparation method and application of heteroatom-doped algae-based charcoal loaded nano zero-valent metal catalyst

    CN115722251A