Martensitic stainless steel for cutting tools and preparation method thereof

By adding Mo and V elements to martensitic stainless steel and adopting specific heat treatment processes, the problem of insufficient toughness of domestic martensitic stainless steel tools is solved, and martensitic stainless steel for tools with high strength and high toughness is prepared. The defect of traditional materials is high in strength but poor in toughness.

CN118685604BActive Publication Date: 2024-11-12TAIYUAN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411181825.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Domestic martensitic stainless steel tools generally face the problem of insufficient toughness, which leads to their high strength but poor toughness, which cannot compete with internationally renowned brands.

Method used

By adding Mo and V elements to the martensite stainless steel and adopting a specific quench-tempering heat treatment process, the obtained martensite stainless steel for tool has good strength and toughness. The specific steps include smelting, hot rolling, spherical annealing, cold rolling and quenching-tempering treatment. The quenching austenitization temperature is 950~1000℃ and the tempering temperature is 240~300℃ to improve the solid solution strengthening of the material and Grain refinement.

Benefits of technology

The martensite stainless steel for cutting tools has a yield strength of 1150~1200MPa, a tensile strength of 1450~1600MPa, an elongation of ≥9.0%, an impact toughness of ≥55J/cm2, and a hardness of 48~50HRC, which overcomes traditional martensite. The problem of high strength but poor toughness of stainless steel has both high strength and high toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118685604B_ABST
    Figure CN118685604B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of martensitic stainless steel, specifically a martensitic stainless steel for cutting tools and a preparation method thereof. A certain amount of Mo and V elements are added to the traditional martensitic stainless steel, which has the effect of solid solution strengthening and grain refinement, and the carbide size and distribution are improved by matching the improved quenching-tempering heat treatment process. The prepared martensitic stainless steel for cutting tools has good strength and toughness. The yield strength of the martensitic stainless steel for cutting tools is 1150~1200MPa, the tensile strength is 1450~1600MPa, the elongation is ≥9.0%, and the impact toughness is ≥55J / cm 2 , hardness is 48~50HRC; the martensitic stainless steel for cutting tools prepared by the present invention overcomes the problems of high strength and poor toughness of previous martensitic stainless steel, has both high strength and high toughness, and has high engineering application value and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of martensitic stainless steel, in particular to martensitic stainless steel for cutting tools and a preparation method thereof. Background Art

[0002] Martensitic stainless steel is widely used in the manufacture of high-performance cutting tools (high-precision professional tools for medical, food processing and military industries), aerospace, mold manufacturing, shipbuilding and other high-end equipment fields due to its high strength, high wear resistance and high corrosion resistance. The products have high added value and large market demand. The materials commonly used for mainstream cutting tools in my country are martensitic stainless steels such as 20Cr13, 30Cr13 and 40Cr13. Compared with the materials used for cutting tools of internationally renowned brands, there is still a certain gap in material quality, and the price is several times or even more than ten times that of foreign countries. Domestic martensitic stainless steel cutting tools generally face the problem of insufficient toughness. Therefore, conducting theoretical research on the strengthening and toughening of martensitic stainless steel and breaking through the key theoretical and technical bottlenecks in the manufacture of martensitic stainless steel cutting tools has high engineering application value and potential economic benefits. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a martensitic stainless steel for cutting tools and a preparation method thereof.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for preparing martensitic stainless steel for cutting tools comprises the following steps:

[0006] S1, smelting and casting to obtain a casting billet;

[0007] S2, hot rolling the ingot to obtain a hot-rolled plate;

[0008] S3, performing spheroidizing annealing on the hot rolled plate;

[0009] S4, cold rolling the annealed hot-rolled sheet to obtain a cold-rolled sheet;

[0010] S5. The cold-rolled sheet is subjected to quenching-tempering treatment, wherein the quenching austenitizing temperature is 950-1000° C., and the holding time is 5-10 min; the quenching method is water cooling; the tempering temperature is 240-300° C., and the holding time is 30-60 min; and the martensitic stainless steel for cutting tools is obtained, wherein the Mo content of the martensitic stainless steel for cutting tools is 0.1-0.4wt%, and the V content is 0.1-0.3wt%.

[0011] As a preferred embodiment of the method for preparing martensitic stainless steel for cutting tools described in the present invention, in step S2, hot rolling is performed in the austenitizing temperature range, the starting rolling temperature is 1150-1200°C, the total reduction is ≥85%, and the hot rolling is followed by air cooling to room temperature.

[0012] As a preferred embodiment of the method for preparing martensitic stainless steel for cutting tools described in the present invention, in step S3, the annealing process is: first, keep warm at 860-890°C for 60-65 minutes, then cool to 590-600°C with the furnace, and then air cool to room temperature.

[0013] As a preferred embodiment of the method for preparing martensitic stainless steel for cutting tools described in the present invention, in step S4, the total cold rolling reduction is 60-70%.

[0014] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0015] A martensitic stainless steel for cutting tools is prepared by adopting the above-mentioned preparation method.

[0016] As a preferred embodiment of the martensitic stainless steel for cutting tools described in the present invention, the composition of the martensitic stainless steel for cutting tools includes, by mass percentage, C: 0.2-0.3%, Cr: 11-14%, Mn: 0.5-1.0%, Si: 0.5-1.0%, Mo: 0.1-0.4%, V: 0.1-0.3%, Ni: 0.2-0.8%, P<0.01%, S<0.01%, and the balance is Fe and unavoidable impurity elements.

[0017] As a preferred embodiment of the martensitic stainless steel for cutting tools of the present invention, the carbide size of the martensitic stainless steel for cutting tools is less than 0.5 μm, and the grain size of the martensitic stainless steel for cutting tools is less than 10 μm.

[0018] As a preferred embodiment of the martensitic stainless steel for cutting tools of the present invention, the yield strength of the martensitic stainless steel for cutting tools is 1150-1200 MPa, the tensile strength is 1450-1600 MPa, the elongation is ≥9.0%, and the impact toughness is ≥55 J / cm 2 , hardness is 48~50HRC.

[0019] The beneficial effects of the present invention are as follows:

[0020] The present invention proposes a martensitic stainless steel for cutting tools and a preparation method thereof. A certain amount of Mo and V elements are added to the traditional martensitic stainless steel, which has the effect of solid solution strengthening and grain refinement, and the carbide size and distribution are improved by matching the improved quenching-tempering heat treatment process. The prepared martensitic stainless steel for cutting tools has good strength and toughness. The yield strength of the martensitic stainless steel for cutting tools is 1150~1200MPa, the tensile strength is 1450~1600MPa, the elongation is ≥9.0%, and the impact toughness is ≥55J / cm 2 , hardness is 48~50HRC; the martensitic stainless steel for cutting tools prepared by the present invention overcomes the problems of high strength and poor toughness of previous martensitic stainless steel, has both high strength and high toughness, and has high engineering application value and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0022] Figure 1 This is the organizational diagram of the martensitic stainless steel for cutting tools prepared in Example 1 of the present invention.

[0023] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0024] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The invention provides a martensitic stainless steel for a tool and a manufacturing method thereof, wherein uniform structure is obtained by adjusting the composition and strictly controlling the heat treatment process, thereby obtaining good mechanical properties, thereby overcoming the problem that the martensitic stainless steel has high strength but poor toughness.

[0026] According to one aspect of the present invention, the present invention provides the following technical solution:

[0027] A method for preparing martensitic stainless steel for cutting tools comprises the following steps:

[0028] S1, smelting and casting to obtain a casting billet;

[0029] S2, hot rolling the ingot to obtain a hot-rolled plate;

[0030] S3, performing spheroidizing annealing on the hot rolled plate;

[0031] S4, cold rolling the annealed hot-rolled sheet to obtain a cold-rolled sheet;

[0032] S5. The cold-rolled sheet is subjected to quenching-tempering treatment, wherein the quenching austenitizing temperature is 950-1000° C., and the holding time is 5-10 min; the quenching method is water cooling; the tempering temperature is 240-300° C., and the holding time is 30-60 min; and the martensitic stainless steel for cutting tools is obtained, wherein the Mo content of the martensitic stainless steel for cutting tools is 0.1-0.4wt%, and the V content is 0.1-0.3wt%.

[0033] The invention adds a certain amount of Mo and V elements to the traditional martensitic stainless steel, which has the effects of solid solution strengthening and grain refinement, and matches the improved quenching-tempering heat treatment process to improve the carbide size and distribution. The prepared martensitic stainless steel for cutting tools has good strength and toughness.

[0034] Preferably, in step S2, the ingot is used as a raw material, and the ingot is heated, hot rolled and pickled to obtain a hot-rolled plate, the heating temperature is 1200-1250°C, hot rolling is performed in the austenitizing temperature range, the start rolling temperature is 1150-1200°C, the total reduction is ≥85%, and the hot rolling is followed by air cooling to room temperature. Specifically, the heating temperature may be, for example, any one of 1200°C, 1210°C, 1220°C, 1230°C, 1240°C, 1250°C, or a range between any two thereof; the start rolling temperature may be, for example, any one of 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, or a range between any two thereof.

[0035] Preferably, in step S3, the annealing process is: first, keep the temperature at 860-890°C for 60-65 minutes, then cool to 590-600°C with the furnace, and then air cool to room temperature. Specifically, the holding temperature can be, for example, any one of 860°C, 870°C, 880°C, 890°C, or a range between any two of them.

[0036] Preferably, in step S4, the total cold rolling reduction is 60-70%. Specifically, the total cold rolling reduction can be, for example, any one of 60%, 62.5%, 65%, 67.5%, 70%, or a range between any two of them.

[0037] Preferably, in step S5, specifically, the austenitizing temperature may be, for example, any one of 950°C, 960°C, 970°C, 980°C, 990°C, 1000°C or a range between any two of them, and the tempering temperature may be, for example, any one of 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C or a range between any two of them.

[0038] According to another aspect of the present invention, the present invention provides the following technical solution:

[0039] A martensitic stainless steel for cutting tools is prepared by adopting the above-mentioned preparation method.

[0040] Preferably, the composition of the martensitic stainless steel for cutting tools includes, by mass percentage, C: 0.2~0.3%, Cr: 11~14%, Mn: 0.5~1.0%, Si: 0.5~1.0%, Mo: 0.1~0.4%, V: 0.1~0.3%, Ni: 0.2~0.8%, P<0.01%, S<0.01%, and the balance is Fe and unavoidable impurity elements.

[0041] C is the main austenitizing element and the main element for improving the hardness and strength of steel. It has strong solid solution strengthening and precipitation strengthening effects. When the carbon content is lower than 0.2wt%, its strength and hardness are relatively low; when the carbon content is higher than 0.3wt%, more chromium carbides are generated, resulting in local chromium-poor points and reduced corrosion resistance of the material. Cr can form an oxide film on the surface of the material, effectively improving the corrosion resistance of the material. To achieve good corrosion resistance, the Cr content should be above 11wt%. At the same time, Cr is also a strong ferrite-forming element. It is easy to form a delta ferrite phase at high temperature, which reduces hot workability. Therefore, its upper limit cannot be higher than 14wt%. Mn is also an austenite-forming element. At the same time, an appropriate amount of Mn can be used as a weak deoxidizer to eliminate the effects of S and O on the hot brittleness of steel. However, too high a Mn content (above 1wt%) will make the steel hard and brittle, which is not conducive to toughness. Too low a Mn content (below 0.5wt%) will weaken its deoxidation and desulfurization effect. Si is a strong deoxidizer and has a solid solution strengthening effect. However, too high a content will lead to poor ductility of steel, and its content should not be greater than 1wt%. Too low a content (below 0.5wt%) will lead to insufficient deoxidation effect. Mo can improve the corrosion resistance of the material, and can also play a role in solid solution strengthening. At the same time, it can improve the hardenability and processability of steel, and can also refine the grains and improve the toughness of steel. When the molybdenum content is lower than 0.1wt%, its strengthening effect is not obvious. On the other hand, molybdenum, as a precious metal, has a comprehensive cost and its role, and its upper limit is 0.4wt%; specifically, the Mo content can be, for example, any one of 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt% or any two of them; V is a strong carbide forming element, and when it reaches more than 0.1wt%, it can refine the grains of the organization and improve the strength and toughness of the steel. However, too high a V content may reduce ductility and toughness, and produce unnecessary primary carbides, and its upper limit is 0.3wt%. Specifically, the V content can be, for example, any one of 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt% or any two thereof; Ni can effectively expand the austenite phase region and improve the stability of austenite, reduce the toughness-brittle transition temperature of steel, and improve the toughness of steel. Its content exceeding the upper limit of 1wt% will lead to an increase in residual austenite and reduce the strength of the material. P and S elements are easy to segregate at the grain boundary, reducing the hot workability of the material, so the lower the content, the better.

[0042] Preferably, the carbide size of the martensitic stainless steel for cutting tools is less than 0.5 μm, and the grain size of the martensitic stainless steel for cutting tools is less than 10 μm; the yield strength of the martensitic stainless steel for cutting tools is 1150-1200 MPa, the tensile strength is 1450-1600 MPa, the elongation is ≥9.0%, and the impact toughness is ≥55 J / cm2 , hardness is 48~50HRC.

[0043] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0044] Example 1

[0045] A method for preparing martensitic stainless steel for cutting tools comprises the following steps:

[0046] S1, smelting and casting to obtain a casting billet;

[0047] S2, using the ingot as a raw material, heating, hot rolling and pickling the ingot to obtain a hot-rolled plate, the heating temperature is 1210° C., hot rolling is performed in the austenitizing temperature range, the starting rolling temperature is 1180° C., the total reduction is 85%, and air cooling is performed to room temperature after hot rolling;

[0048] S3, spheroidizing annealing is performed on the hot-rolled plate; the annealing process is: first, keep the temperature at 890°C for 60 minutes, then cool to 590°C with the furnace, and then air cool to room temperature;

[0049] S4, cold rolling the annealed hot-rolled sheet to obtain a cold-rolled sheet; the total cold-rolling reduction is 62.5%;

[0050] S5, quenching and tempering the cold-rolled sheet, wherein the quenching austenitizing temperature is 990°C and the holding time is 5 minutes; the quenching method is water cooling; the tempering temperature is 250°C and the holding time is 30 minutes; the martensitic stainless steel for cutting tools is obtained. The organization diagram of the martensitic stainless steel for cutting tools prepared in this embodiment is as follows Figure 1 As shown; the composition of martensitic stainless steel for cutting tools is shown in Table 1:

[0051] Table 1 Composition of martensitic stainless steel for cutting tools in Example 1 (mass percentage, wt%)

[0052]

[0053] Example 2

[0054] The difference from Example 1 is that in step S5, the austenitizing temperature is 950°C.

[0055] Comparative Example 1

[0056] The difference from Example 1 is that a commercial 20Cr13 cold-rolled sheet is used.

[0057] Comparative Example 2

[0058] The difference from Example 2 is that a commercial 20Cr13 cold-rolled sheet is used.

[0059] Comparative Example 3

[0060] The difference from Example 1 is that in step S5, the austenitizing temperature is 1030°C.

[0061] Comparative Example 4

[0062] The difference from Example 1 is that in step S5, the tempering temperature is 220°C.

[0063] Comparative Example 5

[0064] The difference from Example 1 is that in step S3, the temperature is kept at 830° C. for 60 minutes.

[0065] Comparative Example 6

[0066] The difference from Example 1 is that the Mo content of the martensitic stainless steel for cutting tools is 0.8 wt %.

[0067] Comparative Example 7

[0068] The difference from Example 1 is that the V content of the martensitic stainless steel for cutting tools is 0.5 wt %.

[0069] Comparative Example 8

[0070] The difference from Example 1 is that the martensitic stainless steel for cutting tools does not contain Mo and V.

[0071] The properties of the martensitic stainless steel obtained in the examples of the present invention and the comparative examples were tested, and the results are shown in Table 2:

[0072] Table 2 Properties of martensitic stainless steel obtained in Examples and Comparative Examples

[0073]

[0074] As can be seen from Table 2, the embodiments of the present invention have better toughness than the comparative examples and can maintain relatively high strength. Figure 1 It can be seen that the structure of the martensitic stainless steel for cutting tools in Example 1 of the present invention is mainly composed of tempered martensite and carbides, the original austenite grains are relatively fine, and the carbides inside them are mainly submicron and nanometer levels and dispersed in the crystals, which effectively reduces the nucleation of microcracks caused by carbides during ductile fracture, ensuring that it has high toughness and strength.

[0075] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing martensitic stainless steel for cutting tools, characterized in that: The steps include: S1, smelting and casting to obtain a casting billet; S2, hot rolling the ingot to obtain a hot-rolled plate; S3, spheroidizing annealing is performed on the hot-rolled plate; the annealing process is: first, keep the temperature at 860-890°C for 60-65min, then cool to 590-600°C with the furnace, and then air-cool to room temperature; S4, cold rolling the annealed hot-rolled sheet to obtain a cold-rolled sheet; S5, performing quenching-tempering treatment on the cold-rolled sheet, wherein the quenching austenitizing temperature is 950-1000° C., and the holding time is 5-10 min; the tempering temperature is 240-300° C., and the holding time is 30-60 min; and the martensitic stainless steel for the tool is obtained; The martensitic stainless steel for cutting tools comprises C: 0.2-0.3%, Cr: 11-14%, Mn: 0.5-1.0%, Si: 0.5-1.0%, Mo: 0.1-0.35%, V: 0.15-0.3%, Ni: 0.2-0.8%, P<0.01%, S<0.01%, and the balance is Fe and unavoidable impurity elements; the yield strength is 1150-1200MPa, the tensile strength is 1450-1600MPa, the elongation is ≥9.0%, and the impact toughness is ≥55J / cm 2 , hardness is 48~50HRC.

2. The method for preparing martensitic stainless steel for cutting tools according to claim 1, characterized in that: In the step S2, hot rolling is performed in the austenitizing temperature range, the starting rolling temperature is 1150-1200° C., the total reduction is ≥85%, and the hot rolling is followed by air cooling to room temperature.

3. The method for preparing martensitic stainless steel for cutting tools according to claim 1, characterized in that: In step S4, the total cold rolling reduction is 60-70%.

4. The method for preparing martensitic stainless steel for cutting tools according to claim 1, characterized in that: In the step S5, the quenching method is water cooling.

5. A martensitic stainless steel for cutting tools, characterized in that: The preparation method is described in any one of claims 1 to 4.

6. The martensitic stainless steel for cutting tools according to claim 5, characterized in that: The carbide size of the martensitic stainless steel for cutting tools is 0.5 μm or less, and the grain size of the martensitic stainless steel for cutting tools is 10 μm or less.