Negative electrode sheet, method for preparing negative electrode sheet and battery

By providing a protective layer and a cross-linking layer on the surface of the metal negative electrode sheet, a composite protective layer is formed by using the cross-linking compound of carboxylic acid ester and amino acid, the problem of dendrites growing and piercing the separator in the battery is solved, and the cycle of the battery is improved Lifespan and safety performance.

CN118693377BActive Publication Date: 2024-12-03JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411188134.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The metal negative electrode in the battery is cracked due to high chemical reactivity and infinite volume changes during the cycle, resulting in the cracking of the SEI film, producing metal dendrites and piercing the diaphragm, causing safety hazards and difficult to inhibit the growth of dendrites.

Method used

The protective layer and the cross-linking layer are provided on the surface of the metal negative electrode sheet, and the cross-linking compound of carboxylic acid ester and amino acid are used to form a composite protective layer, which participates in the formation of the SEI film, enhances the density and stability of the protective layer, and prevents the growth of dendrites and pierce.

Benefits of technology

Effectively inhibit the generation and growth of metal dendrites, improve the cycle life and safety performance of the battery, enhance the protection effect of the metal layer, and prevent dendrites from piercing the diaphragm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118693377B_ABST
    Figure CN118693377B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of battery technology, and provides a negative electrode sheet, a method for preparing the negative electrode sheet, and a battery. The negative electrode sheet includes a metal layer and a protective layer disposed on at least one side of the metal layer, and the area where the metal layer contacts the protective layer forms a junction layer; the metal layer contains a metal substrate, the protective layer contains a first material, and the junction layer contains a second material; the first material includes a first cross-linked product, which is a cross-linked compound of a carboxylic acid ester and an amino acid; the second material includes a second compound, which includes an inorganic end from the metal substrate and an organic end from the first cross-linked product. The negative electrode sheet provided by the present invention can inhibit the growth of metal dendrites and prevent metal dendrites from piercing the diaphragm, thereby improving the cycle life and safety performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a negative electrode sheet, a method for preparing the negative electrode sheet, and a battery. Background Art

[0002] In recent years, a series of emerging metal anodes such as lithium (Li), sodium (Na), potassium (K), zinc (Zn) and aluminum (Al) have attracted widespread attention in high energy density batteries. Among them, metal anodes have obvious practical advantages such as easy availability of raw materials, high cost performance, low redox potential and high specific capacity. However, the practical application of metal anodes is still plagued by the key bottleneck of their high chemical reactivity and unlimited volume change during cycling. Due to the high reactivity and low redox potential of metal anodes, once in contact with the electrolyte, a solid electrolyte interface (SEI) film will form on the metal surface. However, the formed passivation film is usually not strong enough to withstand the volume fluctuation of the metal during the deposition and stripping process, which leads to cracking of the SEI film, resulting in uneven distribution of metal ion flux and the generation of metal dendrites. Continued growth will eventually pierce the separator, causing serious safety hazards.

[0003] Therefore, there is an urgent need to develop a negative electrode sheet that can inhibit the generation and growth of metal dendrites. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art, and to provide a negative electrode sheet, a method for preparing the negative electrode sheet, and a battery. The metal layer surface of the negative electrode sheet of the present invention is provided with a protective layer and a junction layer, and the amino acid in the protective layer and the junction layer can participate in the formation of the SEI film, thereby forming a composite protective layer composed of the junction layer, the protective layer, and the SEI film with the participation of the amino acid, and there is a strong force between the junction layer, the protective layer, and the SEI film with the participation of the amino acid in the composite protective layer, and the composite protective layer is dense, stable, and strong, and forms a good protective effect on the metal layer, thereby inhibiting the growth of metal dendrites, and is also beneficial to prevent metal dendrites from piercing the diaphragm, thereby improving the cycle life and safety performance of the battery.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a negative electrode sheet, which includes a metal layer and a protective layer arranged on the surface of at least one side of the metal layer, and the area where the metal layer and the protective layer are in contact forms a junction layer; the metal layer contains a metal substrate, the protective layer contains a first material, and the junction layer contains a second material; the first material includes a first cross-linked product, which is a cross-linked compound of a carboxylic acid ester and an amino acid; the second material includes a second compound, which includes an inorganic end from the metal substrate and an organic end from the first cross-linked product.

[0006] Optionally, in the first cross-linked product, the mass ratio of the block derived from the carboxylic acid ester to the block derived from the amino acid is (1-6):1.

[0007] Optionally, the carboxylic acid ester is selected from at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate and ethyl propionate.

[0008] Optionally, the amino acid is selected from at least one of proline, tryptophan, serine, tyrosine and glycine.

[0009] Optionally, based on the mass of the first material, the content of the first cross-linked product is 50% by mass to 100% by mass.

[0010] Optionally, the first material further comprises carboxylate and / or amino acid.

[0011] Optionally, based on the mass of the first material, the content of the carboxylic acid ester is 0 mass %-40 mass %.

[0012] Optionally, based on the mass of the first material, the content of the amino acid is 0 mass %-30 mass %.

[0013] Optionally, the organic end derived from the first cross-linked substance is an organic end formed by a carboxylate block in the first cross-linked substance.

[0014] Optionally, the second material also contains components in the first material.

[0015] Optionally, the ratio of the total thickness of the protective layer and the interface layer to the thickness of the metal layer is 1:(1.5-7).

[0016] Optionally, the total thickness of the protective layer and the interface layer is 5µm-50µm.

[0017] Optionally, the thickness of the metal layer is 20µm-80µm.

[0018] The second aspect of the present invention provides a method for preparing the negative electrode sheet according to the first aspect, the method comprising:

[0019] Applying a first slurry on the surface of the metal layer, wherein the first slurry contains a first cross-linked product, and the first cross-linked product is obtained by cross-linking a carboxylate and an amino acid;

[0020] The metal layer contains a metal substrate, and on the surface of the metal layer, the first cross-linked product reacts with the metal substrate to form a junction layer containing a second compound;

[0021] In the area not in contact with the metal layer, the first slurry is dried to form a protective layer.

[0022] Optionally, the conditions of the first reaction include: reaction temperature of 10°C-40°C, and reaction time of 12h-48h.

[0023] Optionally, the method for preparing the first cross-linked product comprises: mixing carboxylic acid ester, amino acid and organic solvent and then performing a second reaction.

[0024] Optionally, the conditions of the second reaction include: reaction temperature of 40°C-60°C, and reaction time of 12h-24h.

[0025] The third aspect of the present invention provides a battery, comprising a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, wherein the negative electrode sheet comprises the negative electrode sheet described in the first aspect and / or the negative electrode sheet obtained by the preparation method described in the second aspect.

[0026] Optionally, in the battery after charge and discharge cycles, a SEI film is also formed on the contact interface between the negative electrode sheet and the electrolyte, and the SEI film contains a third compound and / or a fourth compound, the third compound is obtained by the reaction of the first cross-linked product and the electrolyte, and the fourth compound is obtained by the reaction of the amino acid and the electrolyte.

[0027] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0028] (1) The metal layer of the negative electrode sheet provided by the present invention is provided with a junction layer and a protective layer, which can protect the metal layer and prevent the growth of metal dendrites due to the uncovered part of the metal layer surface. The junction layer is generated by the condensation reaction of the inorganic end of the metal substrate in the metal layer and the organic end of the first cross-linked product in the protective layer, so that the metal layer, the junction layer and the protective layer are more tightly combined, which is more conducive to protecting the metal layer and inhibiting the growth of metal dendrites. In addition, it is also beneficial to prevent metal dendrites from piercing the diaphragm, thereby improving the cycle life and safety performance of the battery.

[0029] (2) The surface of the metal layer on the negative electrode sheet provided by the present invention is coated with a first cross-linked product containing carboxylic acid ester and amino acid, and the first cross-linked product forms a protective layer on the surface of the metal layer to protect the metal layer. The carboxylic acid ester group in the protective layer can undergo a condensation reaction with the metal in the metal layer, thereby forming a junction layer between the metal layer and the protective layer, and the junction layer can further protect the metal layer, and the junction layer makes the metal layer and the protective layer more tightly bonded, which is more conducive to protecting the metal layer. The amino acid group in the protective layer can participate in the formation of the SEI film during the battery assembly charge and discharge, so that the metal layer, the junction layer, the protective layer and the SEI film form a composite protective layer, and the composite protective layer has a strong bonding force with the metal layer. The junction layer, the protective layer and the SEI film in the composite protective layer also have a strong bonding force. Therefore, the composite protective layer formed is dense and stable, not easy to crack, thereby forming a good protective effect on the metal layer, and can inhibit the generation and growth of metal dendrites. Further, it can also inhibit the puncture of the diaphragm by metal dendrites, thereby improving the cycle life and safety of the battery.

[0030] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Shown is a scanning electron microscope image of the negative electrode sheet of the battery in Example 1 after 200 cycles of 1C charge and discharge.

[0032] Figure 2 Shown is a scanning electron microscope image of the negative electrode sheet of the battery in Comparative Example 1 after 200 cycles of 1C charge and discharge. DETAILED DESCRIPTION

[0033] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0034] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0035] The first aspect of the present invention provides a negative electrode sheet, which includes a metal layer and a protective layer arranged on at least one side of the metal layer, and the area where the metal layer and the protective layer are in contact forms a junction layer; the metal layer contains a metal substrate, the protective layer contains a first material, and the junction layer contains a second material; the first material includes a first cross-linked product, which is a cross-linked compound of a carboxylic acid ester and an amino acid; the second material includes a second compound, which includes an inorganic end from the metal substrate and an organic end from the first cross-linked product.

[0036] In the present invention, the metal layer contains a metal substrate, and the metal substrate is selected from at least one of sodium metal, lithium metal and magnesium metal.

[0037] In the present invention, the protective layer contains a first material, the first material includes a first cross-linked product, and the first cross-linked product is a cross-linked compound of carboxylic acid ester and amino acid. In addition, the first material may also include carboxylic acid ester or amino acid that is not involved in the cross-linking.

[0038] In some embodiments, in the first cross-linked product, the mass ratio of the block from carboxylate to the block from amino acid is (1-6):1, for example, 1:1, 2:1, 3:1, 4:1, 5:1 and 6:1. The mass ratio of the block from carboxylate to the block from amino acid is calculated by the following formula: (relative molecular mass of carboxylate block × number of carboxylate blocks) / (relative molecular mass of amino acid block × number of amino acid blocks), and the relative molecular mass and number of blocks can be obtained by techniques such as nuclear magnetic resonance (NMR) or gel permeation chromatography (GPC).

[0039] In some embodiments, based on the mass of the first material, the content of the first cross-linked substance is 50 mass %-100 mass %. When the first material is entirely the first cross-linked substance, the content of the first cross-linked substance is 100 mass %.

[0040] In certain embodiments, the first material further comprises carboxylate and / or amino acid. Carboxylate herein refers to free carboxylate, i.e. when carboxylate reacts with amino acid, the reaction raw material of carboxylate is excessive, and at this time, the first material comprises excessive carboxylate. When the reaction raw material of amino acid is excessive, the first material comprises excessive amino acid.

[0041] In some embodiments, based on the mass of the first material, the content of the carboxylate is 0%-40% by mass, such as 0%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35% and 40% or a range formed by any two endpoints. The content of the carboxylate is the content of excess carboxylate contained in the first material when the reaction raw material of the carboxylate is excessive.

[0042] In some embodiments, the amino acid content is 0%-30% by mass, such as 0%, 1%, 5%, 10%, 15%, 20%, 25% and 30% or a range formed by any two endpoints. The amino acid content is the excess amino acid content in the first material when the amino acid reaction raw material is excessive.

[0043] In some embodiments, the carboxylic acid ester is selected from at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate and ethyl propionate. Preferably, the ethyl acetate is ethyl diazoacetate, and the ethyl formate is ethyl benzoate.

[0044] In some embodiments, the amino acid is selected from at least one of proline, tryptophan, serine, tyrosine, and glycine.

[0045] In the present invention, the interface layer contains a second material, the second material includes a second compound, and the second compound includes an inorganic end derived from the metal substrate and an organic end derived from the first cross-linked product.

[0046] In some embodiments, the interface layer further comprises a product obtained by condensation of an inorganic end of the metal substrate in the metal layer and a carboxylic acid ester in the protective layer that does not participate in the cross-linking reaction.

[0047] In some embodiments, the inorganic end from the metal substrate includes at least one of sodium metal, lithium metal, and magnesium metal.

[0048] In some embodiments, the organic end from the first cross-link is an organic end formed by a carboxylate block in the first cross-link.

[0049] The junction layer is arranged on the surface of the metal layer, which can protect the metal negative electrode, make the passivation film on the surface of the negative electrode sheet more solid, and thus inhibit the growth of metal dendrites. The junction layer is obtained by condensing the metal of the metal substrate in the metal layer and the carboxylate group in the protective layer, so the junction layer can make the metal layer and the protective layer more tightly bonded, denser and more stable.

[0050] In some embodiments, the second material further contains the components of the first material. That is, in addition to the second compound from the condensation reaction of the inorganic end of the metal substrate and the carboxylate group, the second material may also contain a cross-linked compound obtained by the reaction of the carboxylate in the first material and the amino acid, and a carboxylate group or an amino acid group in the first material that does not participate in the cross-linking reaction.

[0051] In some embodiments, the ratio of the total thickness of the protective layer and the junction layer to the thickness of the metal layer is 1:(1.5-7), for example, it can be 1:1.5, 1:2, 1:3, 1:4, 1:5, 1:6 and 1:7. When the ratio of the total thickness of the protective layer and the junction layer to the thickness of the metal layer is 1:(1.5-7), it is beneficial to better form a protective layer on the surface of the metal layer, and it is also beneficial to prevent metal dendrites from piercing the diaphragm, thereby improving the cycle life and safety performance of the battery. When the ratio of the thickness of the metal layer to the total thickness of the protective layer and the junction layer is less than 1.5, the thickness of the metal layer is small, and the thickness of the protective layer and the junction layer is large. At this time, the protective layer and the junction layer can form a good protection for the metal layer to prevent metal dendrites from piercing the diaphragm, but when the thickness is too large, the internal resistance of the battery will increase, affecting the power, rate performance and energy density of the battery. When the thickness of the metal layer is small, the capacity and energy density of the battery are small. When the ratio of the thickness of the metal layer to the total thickness of the protective layer and the junction layer is greater than 7, the thickness of the metal layer is relatively large, the battery capacity is increased, but the metal dendrites are severe, resulting in reduced cycle life and safety performance of the battery. The thickness of the protective layer and the junction layer is relatively small, and cannot provide good protection for the metal layer, and the inhibitory effect on metal dendrites piercing the diaphragm is limited.

[0052] In some embodiments, the total thickness of the protective layer and the interface layer is 5µm-50µm, such as 5µm, 10µm, 15µm, 20µm, 25µm, 30µm, 40µm and 50µm.

[0053] In some embodiments, the thickness of the metal layer is 20µm-80µm, such as 20µm, 30µm, 40µm, 50µm, 60µm, 70µm and 80µm.

[0054] The second aspect of the present invention provides a method for preparing the negative electrode sheet according to the first aspect, the method comprising:

[0055] Applying a first slurry on the surface of the metal layer, wherein the first slurry contains a first cross-linked product, and the first cross-linked product is obtained by cross-linking a carboxylate and an amino acid;

[0056] The metal layer contains a metal substrate, and on the surface of the metal layer, the first cross-linked product reacts with the metal substrate to form a junction layer containing a second compound;

[0057] In the area not in contact with the metal layer, the first slurry is dried to form a protective layer.

[0058] In the present invention, in the area in contact with the metal layer, the carboxylate groups in the first slurry react with the metal in the metal layer to form a junction layer, and the first slurry dries to form a protective layer on the side of the junction layer surface away from the metal layer. There is no obvious interface distinction between the junction layer and the protective layer, and the two form a more dense and strong passivation film on the surface of the metal layer.

[0059] In some embodiments, the preparation method of the first cross-linked product includes: mixing carboxylic acid ester, amino acid and organic solvent to generate a second reaction. The carboxylic acid ester reacts with the amino acid to generate a first cross-linked product. When the first slurry containing the first cross-linked product is coated on the surface of the metal layer, a dense and strong protective layer can be formed on the surface of the metal layer. The protective layer on the surface of the metal layer is not easy to break during the battery cycle, thereby helping to inhibit the growth of metal dendrites and improve the cycle performance and safety performance of the battery.

[0060] In some embodiments, based on the mass of the first slurry, the mass ratio of the added carboxylic acid ester to the added amino acid is (0.5-3):1, such as 0.5:1, 1:1, 2:1 and 3:1. The ester group in the carboxylic acid ester reacts with the hydroxyl group and the amino group in the amino acid. In some embodiments, based on the mass of the first slurry, the content of the added carboxylic acid ester is 5% by mass to 60% by mass, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% by mass and 60% by mass.

[0061] In some embodiments, the conditions of the second reaction include: the reaction temperature is 40°C-60°C, such as 40°C, 45°C, 50°C, 55°C and 60°C, and the reaction time is 12h-24h.

[0062] In some embodiments, the carboxylic acid ester is selected from at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate, and ethyl propionate.

[0063] In some embodiments, the amino acid is selected from at least one of proline, tryptophan, serine, tyrosine, and glycine.

[0064] In some embodiments, the type of the solvent is not limited, and may be at least one of methanol, ethanol, and ethylene glycol.

[0065] In some embodiments, the preparation of the first cross-linked material further comprises adding a catalyst to the reaction raw materials.

[0066] In some embodiments, the catalyst is selected from at least one of boron trifluoride etherate, concentrated phosphoric acid, silicic acid, concentrated sulfuric acid, zinc oxide, stannous chloride and dibutyltin dilaurate.

[0067] In the present invention, when the first slurry is coated on the surface of the metal layer, the first cross-linked product in the first slurry or the free carboxylic acid ester in the first slurry can undergo a first reaction with the metal substrate in the metal layer, thereby forming a junction layer between the metal layer and the protective layer, so the first reaction is a spontaneous condensation reaction.

[0068] In some embodiments, the conditions of the first reaction include: the reaction temperature is 10°C-40°C, such as 10°C, 20°C, 30°C and 40°C, and the reaction time is 12h-48h.

[0069] The third aspect of the present invention provides a battery, comprising a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, wherein the negative electrode sheet comprises the negative electrode sheet described in the first aspect and / or the negative electrode sheet obtained by the preparation method described in the second aspect. The battery may be a sodium metal battery, a lithium metal battery, a potassium metal battery, etc.

[0070] In the present invention, the materials of the positive electrode sheet and the separator are not specifically limited.

[0071] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material coated on the surface thereof, such as the positive electrode active material is Na 0.44 MnO2, Na3V2(PO4)3, Na3V2(PO4)2F3 and Na4Fe3(PO4)2P2O7.

[0072] In some embodiments, the separator may be a conventional separator in the art, for example, the separator is one of a polypropylene separator (PP), a polyethylene separator (PE), a polypropylene / polyethylene double-layer composite film (PP / PE), a polypropylene / polyethylene / polypropylene three-layer composite film (PP / PE / PP), a polyimide electrospinning separator (PI), a cellulose non-woven separator, a polyethylene terephthalate non-woven separator (PET), and a separator with a ceramic coating. The separator is between the positive electrode sheet and the negative electrode sheet to play a role of isolation.

[0073] In some embodiments, the electrolyte includes an organic solvent and a metal salt, and the organic solvent can be at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate, methyl acetate, ethyl propionate, fluoroethylene carbonate, ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, ethylene glycol dimethyl ether, and methyl tert-butyl ether.

[0074] In some embodiments, the metal salt contained in the electrolyte may be a sodium salt, and the sodium salt may be at least one selected from sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate and sodium chloride.

[0075] In some embodiments, in the battery after charge and discharge cycles, a SEI film is also formed on the contact interface between the negative electrode sheet and the electrolyte, and the SEI film contains a third compound and / or a fourth compound, the third compound is obtained by the reaction of the first cross-linked material and the electrolyte, and the fourth compound is obtained by the reaction of the amino acid and the electrolyte. The amino acid in the first cross-linked material in the protective layer or the junction layer can participate in the formation of the SEI film, react to form the third compound, and the free amino acid in the protective layer or the junction layer can also participate in the formation of the SEI film, react to form the fourth compound, and the SEI film contains the third compound and / or the fourth compound, which is conducive to making the SEI film have a stronger bonding force with the junction layer and the protective layer on the surface of the metal layer, forming a better protective effect on the metal layer, and the composite protective layer formed by the junction layer, the protective layer and the SEI film on the surface of the metal layer is more compact and stable, which can inhibit the growth of metal dendrites and improve the cycle life and safety of the metal battery.

[0076] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0077] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0078] The present invention is described in detail below in conjunction with specific examples, which are used to understand but not to limit the present invention. In the following examples, 1 part represents 1 g.

[0079] Example 1

[0080] This example is used to illustrate the preparation of the negative electrode sheet of the present invention.

[0081] (1) 8.5 parts of ethyl acetate, 6.5 parts of tyrosine, 4 parts of boron trifluoride etherate and 15 parts of methanol were mixed and reacted for 24 hours with the reaction temperature controlled at 40°C. After the reaction time was over, the mixture was heated to 100°C and the trace amount of water in the solution was removed for 30 minutes. Finally, the mixture was transferred to a glove box (water and oxygen were controlled to be less than 0.1 ppm) to obtain a first slurry. The ethyl acetate in the first slurry reacted with tyrosine to generate a first cross-linked product.

[0082] The first slurry was tested by quantitative infrared spectroscopy and the content of ethyl acetate and tyrosine crosslinking was 93.5%. The mass ratio of the ethyl acetate block to the tyrosine block was 3:1.

[0083] (2) Place the sodium sheet on the sample plate in the glove box, and use a small cotton brush to dip the first slurry and evenly apply it on the surface of the sodium metal sheet to obtain a protective layer. After standing for 12 hours, the acetate groups in the first slurry undergo a self-condensation reaction on the surface of the sodium metal, and a junction layer is formed between the sodium metal sheet and the protective layer. The thickness of the metal layer is 50 μm, and the total thickness of the protective layer and the junction layer is 10 μm.

[0084] (3) The sodium metal sheet in step 2 is assembled into a battery with a positive electrode shell, a positive electrode sheet, a separator, an electrolyte, a gasket and a negative electrode shell. During the battery charging and discharging process, the amino acid molecules in the interface layer and the protective layer on the surface of the sodium metal sheet can participate in the formation of the SEI film, making the SEI film have better density and stability.

[0085] Example 2

[0086] This example is used to illustrate the preparation of negative electrode sheets with different mass fractions of carboxylic acid ester and amino acid.

[0087] Example 2-1

[0088] The operation was carried out according to the method described in Example 1, except that the ratio of ethyl acetate to tyrosine was changed but the total mass fraction of ethyl acetate and tyrosine was kept unchanged, specifically, 10 parts of ethyl acetate and 5 parts of tyrosine. The thickness of the metal layer was 50 μm, and the total thickness of the protective layer and the interface layer was 10 μm. The mass ratio of the block of ethyl acetate to the block from the tyrosine was 6:1.

[0089] Example 2-2

[0090] The operation was carried out according to the method described in Example 1, except that the ratio of ethyl acetate to tyrosine was changed but the total mass fraction of ethyl acetate and tyrosine was kept unchanged, specifically, 9 parts of ethyl acetate and 6 parts of tyrosine. The thickness of the metal layer was 50 μm, and the total thickness of the protective layer and the interface layer was 10 μm. The mass ratio of the block of ethyl acetate to the block from the tyrosine was 4:1.

[0091] Example 2-3

[0092] The operation was carried out according to the method described in Example 1, except that the ratio of ethyl acetate to tyrosine was changed but the total mass fraction of ethyl acetate and tyrosine was kept unchanged, specifically, 5 parts of ethyl acetate and 10 parts of tyrosine. The thickness of the metal layer was 50 μm, and the total thickness of the protective layer and the interface layer was 10 μm. The mass ratio of the block of ethyl acetate to the block from the tyrosine was 1:1.

[0093] Embodiment 2-4

[0094] The operation was carried out according to the method described in Example 1, except that the ratio of ethyl acetate to tyrosine was changed but the total mass fraction of ethyl acetate and tyrosine was kept unchanged, specifically, 8 parts of ethyl acetate and 7 parts of tyrosine. The thickness of the metal layer was 50 μm, and the total thickness of the protective layer and the interface layer was 10 μm. The mass ratio of the block of ethyl acetate to the block from the tyrosine was 2:1.

[0095] Example 3

[0096] This example is used to illustrate the preparation of negative electrode sheets when different carboxylic acid esters and amino acids are selected.

[0097] Example 3-1

[0098] The procedure described in Example 1 was followed, except that ethyl diazoacetate was used instead of ethyl acetate.

[0099] Example 3-2

[0100] The procedure was followed as described in Example 1, except that proline was used instead of tyrosine.

[0101] Example 4

[0102] This embodiment is used to illustrate the preparation of a negative electrode sheet when the ratio of the sum of the thickness of the protective layer and the junction layer to the thickness of the metal layer is different.

[0103] Example 4-1

[0104] The operation was carried out according to the method described in Example 1, except that the sum of the thickness of the protective layer and the interface layer was 6 μm.

[0105] Example 4-2

[0106] The operation was carried out according to the method described in Example 1, except that the sum of the thickness of the protective layer and the interface layer was 30 μm.

[0107] Example 4-3

[0108] The operation was carried out according to the method described in Example 1, except that the sum of the thickness of the protective layer and the interface layer was 2 μm.

[0109] Comparative Example 1

[0110] This comparative example is used to illustrate the preparation of a negative electrode sheet when no interface layer and protective layer are provided on the surface of the metal sodium sheet.

[0111] The method described in Example 1 was followed, except that the metal sodium sheets not coated with the first slurry were directly used to assemble the battery.

[0112] Comparative Example 2

[0113] This comparative example is used to illustrate the preparation of a negative electrode sheet when the protective layer coated on the surface of the metal sodium sheet does not contain amino acids.

[0114] The method described in Example 1 was followed, except that the tyrosine in step (1) was replaced by the same weight portion of ethyl acetate.

[0115] Comparative Example 3

[0116] This comparative example is used to illustrate the preparation of a negative electrode sheet when the protective layer coated on the surface of the metal sodium sheet does not contain ethyl acetate.

[0117] The method described in Example 1 was followed, except that the ethyl acetate in step (1) was replaced with the same weight portion of tyrosine.

[0118] Comparative Example 4

[0119] This comparative example is used to illustrate the preparation of a negative electrode sheet when the surface of the metal sodium sheet is coated with a cross-linked product other than ethyl acetate-amino acid.

[0120] The method described in Example 1 was followed, except that ethyl acetate was coated on the surface of the metal sodium sheet, and then the amino acid slurry was coated on the surface of the ethyl acetate coating.

[0121] Test Case

[0122] Preparation of positive electrode sheet: Sodium nickel cobalt manganese oxide, conductive carbon black SP, binder PVDF (polyvinylidene fluoride) are mixed in a ratio of 95:2:3 with an appropriate amount of NMP (N-methylpyrrolidone) to prepare a positive electrode slurry, which is coated on aluminum foil, dried at 100°C, and pressed into a positive electrode sheet by a tablet press.

[0123] Electrolyte: 1 mol / L sodium hexafluorophosphate, ethylene carbonate: dimethyl carbonate: diethanol dimethyl ether are prepared in a mass ratio of 2:4:1 to form a sodium metal battery electrolyte.

[0124] (1) Scanning electron microscopy (SEM): 25°C, battery 1C charge and discharge, disassemble the battery after 200 cycles, and take the negative electrode sheet for SEM photography.

[0125] (2) Cycle test: At 25°C, charge the battery at 1C constant current and constant voltage to 4.0V. After standing for 30 minutes, discharge at 1C to 2.0V and record the cycle number.

[0126] (3) 1000-cycle capacity retention rate: 1. Take the battery after capacity division and first charge it to 4.25V with a constant current of 1C, and then charge it to I≤0.05C with a constant voltage of 4.25V; 2. After standing for 5 minutes, discharge the battery to 2.8V with a constant current of 1C to obtain the discharge capacity C1; 3. Stand for 30 minutes. Repeat steps 1-3 999 times to obtain the discharge capacity C1000; the 1000-cycle capacity retention rate is calculated as (C1000) / (C1)*100%.

[0127]

[0128] Figure 1 The figure shows a scanning electron microscope image of the negative electrode sheet after 200 cycles of 1C charge and discharge of the battery in Example 1. It can be seen from the figure that the surface of the negative electrode sheet is dense, that is, the composite protective layer on the surface of the negative electrode metal layer is dense and strong, which can form a good protection effect on the metal layer and inhibit the growth of metal dendrites.

[0129] Figure 2 The figure shows a scanning electron microscope image of the negative electrode sheet of the battery 1C in comparative example 1 after 200 cycles of charge and discharge. It can be seen from the figure that the surface of the negative electrode sheet is relatively loose, and the protective layer on the surface of the negative electrode sheet is prone to cracks after multiple cycles, which makes it easy to grow lithium dendrites and the electrolyte reacts harmfully with metallic lithium, further consuming the lithium metal, which is more conducive to the growth of more lithium dendrites.

[0130] It can be seen from the data of the above embodiments and comparative examples that the number of cycles and the 1000-cycle capacity retention rate of the battery prepared by the negative electrode sheet of the present invention are much greater than those of the battery prepared by the negative electrode sheet in the comparative example. Compared with the negative electrode sheet in the comparative example whose metal layer surface is not coated with a cross-linked compound containing carboxylate and amino acid, the negative electrode sheet of the present invention coated with a cross-linked compound containing carboxylate and amino acid does help to inhibit metal dendrites and improve the cycle life of the battery.

[0131] The negative electrode sheet of the embodiment of Table 1 is a cross-linked compound containing carboxylate and amino acid coated on the surface of the metal layer. The cross-linked compound formed by carboxylate and amino acid can form a protective layer on the metal layer, and the carboxylate in the protective layer and the metal layer can react between the metal layer and the protective layer to form a junction layer. The amino acid in the protective layer and the junction layer can also participate in the formation of the SEI film, thereby forming a composite protective layer composed of the junction layer, the protective layer and the SEI film with the participation of amino acid. The negative electrode sheet of the comparative example is not coated on the surface of the metal layer or only coated with carboxylate or only coated with amino acid or coated with a substance that carboxylate and amino acid are not cross-linked. The number of cycles and capacity retention rate of the comparative example are far worse than those of the embodiment, so the composite protective layer of the present invention can form a good protective effect on the metal layer, thereby inhibiting the growth of metal dendrites, and is also beneficial to prevent metal dendrites from piercing the diaphragm, thereby improving the cycle life and safety performance of the battery.

[0132] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A negative electrode sheet, characterized in that: The negative electrode sheet comprises a metal layer and a protective layer disposed on at least one side of the metal layer, wherein the area where the metal layer contacts the protective layer forms a junction layer; the metal layer comprises a metal substrate, the protective layer comprises a first material, and the junction layer comprises a second material; the first material comprises a first cross-linked product, and the first cross-linked product is a cross-linked compound of a carboxylic acid ester and an amino acid; The second material includes a second compound, the second compound including an inorganic end from the metal substrate and an organic end from the first cross-linked product; The metal substrate is selected from at least one of sodium metal, lithium metal and magnesium metal; The carboxylic acid ester is selected from at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate and ethyl propionate; The amino acid is selected from at least one of proline, tryptophan, serine, tyrosine and glycine.

2. The negative electrode sheet according to claim 1, characterized in that: In the first cross-linked product, the mass ratio of the block derived from the carboxylate to the block derived from the amino acid is (1-6):

1.

3. The negative electrode sheet according to claim 2, characterized in that: Based on the mass of the first material, the content of the first cross-linked product is 50 mass %-100 mass %.

4. The negative electrode sheet according to claim 2, characterized in that: The first material also includes carboxylic acid esters and / or amino acids.

5. The negative electrode sheet according to claim 4, characterized in that: Based on the mass of the first material, the content of the carboxylic acid ester is 0 mass % to 40 mass %; and / or, Based on the mass of the first material, the content of the amino acid is 0 mass %-30 mass %.

6. The negative electrode sheet according to claim 1, characterized in that: The organic end derived from the first cross-linked product is an organic end formed by the block derived from the carboxylate in the first cross-linked product; and / or, The second material further contains the components of the first material.

7. The negative electrode sheet according to claim 1, characterized in that: The ratio of the total thickness of the protective layer and the interface layer to the thickness of the metal layer is 1:(1.5-7); and / or, The total thickness of the protective layer and the interface layer is 5µm-50µm; and / or, The thickness of the metal layer is 20µm-80µm.

8. A method for preparing the negative electrode sheet according to any one of claims 1 to 7, characterized in that: The method includes: Applying a first slurry on the surface of the metal layer, wherein the first slurry contains a first cross-linked product, and the first cross-linked product is obtained by cross-linking a carboxylate and an amino acid; The metal layer contains a metal substrate, and on the surface of the metal layer, the first cross-linked product reacts with the metal substrate to form a junction layer containing a second compound; In the area not in contact with the metal layer, the first slurry is dried to form a protective layer.

9. The method according to claim 8, characterized in that The preparation method of the first cross-linked product comprises: The second reaction occurs after the carboxylic acid ester, amino acid and organic solvent are mixed.

10. The method according to claim 9, characterized in that The conditions of the first reaction include: reaction temperature of 10°C-40°C, reaction time of 12h-48h; and / or, The conditions of the second reaction include: reaction temperature of 40°C-60°C, and reaction time of 12h-24h.

11. A battery, characterized in that: The invention comprises a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, wherein the negative electrode sheet comprises the negative electrode sheet according to any one of claims 1 to 7 and / or the negative electrode sheet obtained by the preparation method according to any one of claims 8 to 10.

12. The battery according to claim 11, characterized in that In the battery after charge and discharge cycles, a SEI film is also formed on the contact interface between the negative electrode sheet and the electrolyte, and the SEI film contains a third compound and / or a fourth compound, the third compound is obtained by the reaction of the first cross-linked product and the electrolyte, and the fourth compound is obtained by the reaction of the amino acid and the electrolyte.