High-temperature-resistant and salt-resistant gel modifying and flooding agent and preparation method thereof
Through the combination of modified polyacrylamide and modified bentonite, the durability problem of the polymer conditioning and flooding agent under high temperature and high salt conditions is solved, and the high temperature resistance, salt resistance and expansion performance of the gel conditioning and flooding agent are realized, and the performance of the gel conditioning and flooding agent is improved. It improves oil recovery, simplifies the preparation process, and is suitable for large-scale production.
Patent Information
- Application Number
- CN202410709195.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-09-27
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing technology, polymer control and displacement agents are not durable under high-temperature and high-salt conditions, resulting in low oil recovery rates. Moreover, the preparation process of existing control and displacement agents is complex and difficult to produce on a large scale.
A gel conditioning and displacing agent combining modified polyacrylamide and modified bentonite is used to enhance the high temperature resistance and salt resistance of the polymer by adding amide groups and introducing sulfonic acid groups, and changing its structure through modified bentonite. Improve water blocking effect.
It achieves good high temperature resistance, salt resistance and expansion performance of the gel control and displacement agent, improves oil recovery, simplifies the preparation process, and is suitable for large-scale production.
Smart Images

Figure BDA0004873509400000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of profile control, water plugging and oil displacement, and in particular to a high temperature resistant and salt resistant gel displacement agent and a preparation method thereof. Background Art
[0002] Oil is an important strategic resource. With the development of economy and science and technology, the demand for oil is increasing. At present, the water drive recovery rate of most oil fields in my country is low, and further oil production is needed, so polymer flooding technology is produced accordingly. Through field investigation, remaining oil evaluation and water injection development recovery rate analysis of most oil fields in my country, it is determined that polymer flooding is the main direction of tertiary oil recovery in the near future. The application of polymer flooding technology can effectively improve the viscosity difference between oil and displacement fluid, improve mobility ratio and increase swept volume. Polymer flooding technology has been developed into gel flooding technology in combination with deep reservoir flooding and is widely used. At present, polymer flooding is applied to reservoirs with high temperature and high mineralization. Therefore, the development of a flooding polymer system with temperature and salt resistance is of great significance to the development of my country's petroleum industry.
[0003] Patent No. CN115873570A discloses a microbial oil recovery and profile control agent and its application in oil reservoir water plugging and profile control. The invention includes: microbial fermentation liquid; auxiliary denaturant; the rest is water. The beneficial effects of the invention are: (1) The microbial oil recovery and profile control agent provided by the present invention has the advantages of low cost, simple configuration, and no need for special equipment and processes; it has the effect of reducing pressure and increasing injection during injection, and after injection, it denatures in the deep part of the oil reservoir to become a high-efficiency profile control agent, and is gradually degraded by formation microorganisms, without formation blockage and environmental pollution. Problems; (2) The profile control agent of the invention is injected on-site in multiple rounds of slugs to achieve efficient use of the remaining oil in different oil recovery in the oil reservoir, with an effective period of more than 5 years, and an increase in recovery rate of more than 15%. However, microorganisms have strict requirements on the environment and limited production, so the profile control agent is not suitable for large-scale production.
[0004] The patent invention with patent number CN112708405B discloses an integrated profile control agent and its preparation method and application. The profile control agent includes: modified montmorillonite plugging agent, surfactant, nano-active agent, additive and water; the integrated profile control agent provided by the invention can expand the water drive swept volume, improve the oil washing efficiency, and also has the function of plugging and oil washing. The preparation method of the integrated profile control agent of the invention is simple, and it can be prepared in a short time at room temperature. It solves the practical problems of the complex preparation process of the existing profile control agent and the difficulty of on-site construction. It has important significance and economic value for improving the effect of water drive development and achieving water control and oil stabilization in oil fields. However, the profile control agent with montmorillonite as the main material may cause seepage.
[0005] In view of the current technical problems, it is of practical significance to develop a high temperature and salt resistant gel flooding agent and its preparation method. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a high temperature resistant and salt resistant gel flooding agent and a preparation method thereof. The preparation process of the gel flooding agent of the present invention is simple, and no complicated production and processing is required, which can greatly save production time. The gel flooding agent has good high temperature resistance, salt resistance and excellent expansion performance.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] The first aspect of the present invention provides a high temperature resistant and salt resistant gel displacement agent, which comprises the following raw materials in parts by weight: 1-1.3 parts of modified polyacrylamide, 0.05-0.15 parts of composite cross-linking agent, 40-50 parts of modified bentonite, 0.5-1 parts of surfactant, 0.1-0.2 parts of stabilizer, and 120-150 parts of water.
[0009] In some embodiments, the modified polyacrylamide comprises the following preparation steps:
[0010] (1) completely dissolving acrylamide, N,N-methylenebisacrylamide, acrylic acid, poly(2-acrylamide-2-methyl-1-propanesulfonic acid) and ammonium persulfate in water to form a solution A;
[0011] (2) adding N,N,N,N-tetramethylethylenediamine to the solution A of step (1) to form a reaction solution B;
[0012] (3) placing the reaction solution B in step (2) in a vacuum reactor at 60-70° C. for 8-10 hours to obtain a reaction solution C;
[0013] (4) adding isopropanol to the reaction solution C of step (3) to generate a precipitate, which is filtered and dried to obtain the modified polyacryloyl.
[0014] Preferably, the modified polyacrylamide comprises the following preparation steps:
[0015] (1) completely dissolving acrylamide, N,N-methylenebisacrylamide, acrylic acid, poly(2-acrylamide-2-methyl-1-propanesulfonic acid) and ammonium persulfate in water to form a solution A;
[0016] (2) adding N,N,N,N-tetramethylethylenediamine to the solution A of step (1) to form a reaction solution B;
[0017] (3) placing the reaction solution B in step (2) in a vacuum reactor at 65° C. for 9 h to obtain a reaction solution C;
[0018] (4) adding isopropanol to the reaction solution C of step (3) to generate a precipitate, which is filtered and dried to obtain the modified polyacryloyl.
[0019] Polyacrylamide and its derivatives have been widely used in crude oil production. As the main agent of polymer flooding, polyacrylamide can increase the overall viscosity of the flooding system, increase the force of the oil-water interface on crude oil, and expand the sweep coefficient of the flooding system, thereby reducing the residual rate of crude oil and increasing the recovery rate of crude oil. However, polyacrylamide has poor temperature and salt resistance. Under high-temperature hydrolysis conditions, its molecular chain will curl and its viscosity will decrease. Under reservoir conditions, the maximum applicable temperature of polyacrylamide is 75°C. Under high mineralization conditions, the viscosity of polyacrylamide aqueous solution decreases rapidly, and high content of divalent metal ions may even cause it to precipitate or even lose viscosity.
[0020] The applicant increases the proportion of amide groups and introduces sulfonic acid groups. The various hydrophilic groups contained in the polymer make the molecules more stretched in water, enhance the viscosity of the polymer at high temperatures, and make the displacement agent have good high temperature resistance. In addition, the sulfonic acid groups are less affected by divalent metal ions in water. Therefore, the modified polyacrylamide can enhance the salt resistance of the displacement agent.
[0021] In some embodiments, the molar ratio of acrylamide, N,N-methylenebisacrylamide, acrylic acid and poly(2-acrylamide-2-methyl-1-propanesulfonic acid) is 1:(1-2):(1-3):(1-2).
[0022] Preferably, the molar ratio of acrylamide, N,N-methylenebisacrylamide, acrylic acid and poly(2-acrylamide-2-methyl-1-propanesulfonic acid) is 1:1:1:1.
[0023] In some embodiments, the relative molecular weight of the modified polyacrylamide is ≧14 million.
[0024] In some embodiments, the modified bentonite comprises the following preparation steps:
[0025] After bentonite, poly (2-acrylamide-2-methyl-1-propanesulfonic acid) and di-tert-butyl peroxide are mixed and stirred at 50-70° C. for 2-3 hours, the temperature is raised to 110-140° C. and stirred at high speed for 1-2 hours before discharging the material to obtain poly (2-acrylamide-2-methyl-1-propanesulfonic acid) modified bentonite.
[0026] Preferably, the modified bentonite comprises the following preparation steps:
[0027] Bentonite, poly (2-acrylamide-2-methyl-1-propanesulfonic acid) and di-tert-butyl peroxide were mixed and stirred at 60°C for 2 hours, and then the temperature was raised to 110°C and stirred at high speed for 1.5 hours before discharging the material to obtain poly (2-acrylamide-2-methyl-1-propanesulfonic acid) modified bentonite.
[0028] Bentonite can swell in water and is often used as a water plugging agent in oil production. However, bentonite has a loose structure after adding water and its water plugging effect is limited.
[0029] The applicant found that by mixing and copolymerizing bentonite with poly (2-acrylamide-2-methyl-1-propanesulfonic acid), when the bentonite swells in water, the polymer can block the pores therein, reducing the water permeability, thereby improving the water blocking effect. At the same time, the heteroatoms in the polymer can change the surface and interlayer structure of the bentonite, so that the displacement agent has good expansion performance, salt resistance and high temperature resistance.
[0030] In some embodiments, the mass ratio of the bentonite, poly(2-acrylamide-2-methyl-1-propanesulfonic acid) and di-tert-butyl peroxide is 100:(12-20):(0.13-0.2).
[0031] Preferably, the mass ratio of the bentonite, poly(2-acrylamide-2-methyl-1-propanesulfonic acid) and di-tert-butyl peroxide is 100:15:0.15.
[0032] In some embodiments, the composite cross-linking agent is resorcinol and benzaldehyde.
[0033] Preferably, the molar ratio of the composite cross-linking agent resorcinol to benzaldehyde is 1:(2-3).
[0034] Further preferably, the molar ratio of the composite cross-linking agent resorcinol to benzaldehyde is 1:2.2.
[0035] In some embodiments, the surfactant is one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium bromide, α-olefin sulfonate, and petroleum sulfonate.
[0036] Preferably, the surfactant is sodium petroleum sulfonate.
[0037] In some embodiments, the stabilizer is one or more of sodium thiosulfate, thiourea, 2,4-dithiobiuret, semicarbazide, thiosemicarbazide, 1,4-phenylenebis(thiourea), and sodium polyphosphate.
[0038] Preferably, the stabilizer is thiourea.
[0039] Another aspect of the present invention provides a method for preparing a high temperature resistant and salt resistant gel flooding agent, comprising the following steps:
[0040] S1. Mix and stir 120-150 parts of water, 40-50 parts of modified bentonite, 0.5-1 parts of surfactant and 1-1.3 parts of modified polyacrylamide to obtain a mixture A;
[0041] S2, adding 0.1-0.2 parts of stabilizer to mixture A and stirring for 20-30 minutes to obtain mixture B;
[0042] S3, adding 0.05-0.15 parts of a composite crosslinking agent to the mixture B in S2 and stirring for 30-40 minutes to obtain a mixture C;
[0043] S4. Place the mixture C in S3 in a constant temperature box at 100-130° C. to react for 5-7 days to obtain a gel displacement agent.
[0044] Preferably, the method for preparing the high temperature and salt resistant gel flooding agent comprises the following steps:
[0045] S1, 140 parts of water, 47 parts of modified bentonite, 0.7 parts of surfactant and 1.1 parts of modified polyacrylamide were mixed and stirred to obtain a mixture A;
[0046] S2, adding 0.15 parts of stabilizer to mixture A and stirring for 20 minutes to obtain mixture B;
[0047] S3, adding 0.12 parts of the composite crosslinking agent to the mixture B in S2 and stirring for 30 minutes to obtain a mixture C;
[0048] S4, placing the mixture C in S3 in a constant temperature box at 120°C for reaction for 5 days to obtain a gel drive agent. Compared with the prior art, the beneficial effects of the present invention are:
[0049] 1. The gel displacement agent of the present invention is easy to prepare, has good plugging effect and salt and high temperature resistance, and can effectively improve oil recovery rate.
[0050] 2. The homemade modified polyacrylamide of the present invention is rich in a variety of hydrophilic groups, which makes the modified polyacrylamide molecules more stretchable in high-salt and high-temperature mineral water, and has good salt and high-temperature resistance; at the same time, the N, O, and S heteroatoms in the molecules can make the combination of the control and displacement agent and the rock wall tighter, and the water plugging effect is better.
[0051] 3. The homemade modified bentonite of the present invention changes the surface and interlayer structure of the bentonite, and the water permeability is weakened, so that the displacement agent has good expansion performance, water blocking performance and salt and high temperature resistance. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0053] In order to better illustrate the specific implementation of the present invention, the following examples are further illustrated. The weight parts described in the following examples are in grams, that is, 1 weight part is 1g.
[0054] The bentonite used in the examples and comparative examples of the present invention was purchased from Weifang Huawei New Material Technology Co., Ltd. The polyacrylamide used was purchased from Henan Saike Environmental Protection Technology Co., Ltd.
[0055] Preparation Example 1
[0056] The preparation method of modified polyacrylamide comprises the following steps:
[0057] (1) 10 g of acrylamide, 22 g of N,N-methylenebisacrylamide, 10 g of acrylic acid, 29 g of poly(2-acrylamide-2-methyl-1-propanesulfonic acid) and 0.65 g of ammonium persulfate were completely dissolved in water to form a solution A;
[0058] (2) adding 0.33 g of N,N,N,N-tetramethylethylenediamine to the solution A of step (1) to form a reaction solution B;
[0059] (3) placing the reaction solution B in step (2) in a vacuum reactor at 65° C. for 9 h to obtain a reaction solution C;
[0060] (4) Add 1000 mL of isopropanol to the reaction solution C of step (3) to generate a precipitate, which is filtered and dried to obtain the modified polyacrylamide.
[0061] Preparation Example 2
[0062] The preparation method of modified polyacrylamide is the same as that of Preparation Example 1, except that the mass of the used N,N-methylenebisacrylamide is 70 g.
[0063] Preparation Example 3
[0064] The preparation method of modified polyacrylamide is the same as that of Preparation Example 1, except that the mass of the used poly(2-acrylamide-2-methyl-1-propanesulfonic acid) is 76 g.
[0065] Preparation Example 4
[0066] The preparation method of modified bentonite comprises the following steps:
[0067] 100 g of bentonite, 15 g of poly (2-acrylamide-2-methyl-1-propanesulfonic acid) and 0.15 g of di-tert-butyl peroxide were mixed and stirred at 60 ° C for 2 hours, and then the temperature was raised to 110 ° C and stirred at high speed for 1.5 hours before discharging the material to obtain poly (2-acrylamide-2-methyl-1-propanesulfonic acid) modified bentonite.
[0068] Preparation Example 5
[0069] The preparation method of modified bentonite is the same as that of Preparation Example 4, except that the mass of the bentonite used is 150 g.
[0070] Example 1
[0071] The present embodiment provides a high temperature resistant and salt resistant gel displacement agent, which includes the following raw materials in parts by weight: 1.1 parts of modified polyacrylamide, 0.12 parts of a composite cross-linking agent (including resorcinol and benzaldehyde in a molar ratio of 1:2.2), 47 parts of modified bentonite, 0.7 parts of sodium petroleum sulfonate, 0.15 parts of thiourea, and 140 parts of water.
[0072] Among them, the modified polyacrylamide is prepared by Preparation Example 1; and the modified bentonite is prepared by Preparation Example 5.
[0073] S1. Mix water, modified bentonite, sodium petroleum sulfonate and modified polyacrylamide and stir them uniformly to obtain a mixture A;
[0074] S2, adding thiourea to mixture A and stirring for 20 minutes to obtain mixture B;
[0075] S3, adding resorcinol and benzaldehyde to the mixture B in S2 and stirring for 30 minutes to obtain a mixture C;
[0076] S4. Place the mixture C in S3 in a constant temperature box at 120° C. for reaction for 6 days to obtain a gel displacement agent.
[0077] Example 2
[0078] The present embodiment provides a high temperature and salt resistant gel displacement agent, which includes the following raw materials in parts by weight: 1 part of modified polyacrylamide, 0.05 parts of a composite cross-linking agent (including resorcinol and benzaldehyde in a molar ratio of 1:2), 40 parts of modified bentonite, 0.5 parts of sodium petroleum sulfonate, 0.1 parts of thiourea, and 120 parts of water.
[0079] Among them, the modified polyacrylamide is prepared by Preparation Example 1; and the modified bentonite is prepared by Preparation Example 5.
[0080] S1. Mix water, modified bentonite, sodium petroleum sulfonate and modified polyacrylamide and stir them uniformly to obtain a mixture A;
[0081] S2, adding thiourea to mixture A and stirring for 20 minutes to obtain mixture B;
[0082] S3, adding resorcinol and benzaldehyde to the mixture B in S2 and stirring for 30 minutes to obtain a mixture C;
[0083] S4. Place the mixture C in S3 in a constant temperature box at 100° C. to react for 7 days to obtain a gel displacement agent.
[0084] Example 3
[0085] The present embodiment provides a high temperature and salt resistant gel displacement agent, which includes the following raw materials in parts by weight: 1.3 parts of modified polyacrylamide, 0.15 parts of a composite cross-linking agent (including resorcinol and benzaldehyde in a molar ratio of 1:3), 50 parts of modified bentonite, 1 part of sodium petroleum sulfonate, 0.2 parts of thiourea, and 150 parts of water.
[0086] Among them, the modified polyacrylamide is prepared by Preparation Example 1; and the modified bentonite is prepared by Preparation Example 5.
[0087] S1. Mix water, modified bentonite, sodium petroleum sulfonate and modified polyacrylamide and stir them uniformly to obtain a mixture A;
[0088] S2, adding thiourea to mixture A and stirring for 30 minutes to obtain mixture B;
[0089] S3, adding resorcinol and benzaldehyde to the mixture B in S2 and stirring for 40 minutes to obtain a mixture C;
[0090] S4. Place the mixture C in S3 in a constant temperature box at 130° C. for reaction for 5 days to obtain a gel displacement agent.
[0091] Example 4
[0092] This embodiment provides a high temperature resistant and salt resistant gel displacement agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified polyacrylamide is prepared by Preparation Example 2.
[0093] Example 5
[0094] This embodiment provides a high temperature resistant and salt resistant gel displacement agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified polyacrylamide is prepared by Preparation Example 3.
[0095] Example 6
[0096] This embodiment provides a high temperature resistant and salt resistant gel displacement agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified bentonite is prepared by Preparation Example 5.
[0097] Comparative Example 1
[0098] This comparative example provides a high temperature resistant and salt resistant gel displacement agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of polyacrylamide is used instead of modified polyacrylamide.
[0099] Comparative Example 2
[0100] This comparative example provides a high temperature resistant and salt resistant gel displacement agent and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of bentonite is used instead of modified bentonite.
[0101] Performance test of gel flooding agent
[0102] (1) Expansion performance test: The performance of the displacement agent is evaluated by the expansion ratio of the displacement agent. The expansion ratio is calculated by the following formula: expansion ratio = (M2-M1) / M1, where: M1 = the mass of the displacement agent before water absorption (g), M2 = the mass of the displacement agent after water absorption (g);
[0103] (2) Viscosity test: At 95°C, the total mineralization of the brine is 180,000 mg / L, of which Ca 2+ +Mg 2+ The content of 5000mg / L was measured by Haake rheometer at a concentric cylinder shear rate of 7.34s -1 Under the conditions of , the viscosity of 1000 mg / L of the displacement agent aqueous solution and the apparent viscosity of the displacement agent aqueous solution after aging at 95°C for 30 days were tested.
[0104] Table 1
[0105]
[0106] As can be seen from Table 1, the apparent viscosity, apparent viscosity after 30 days and expansion multiple of the gel displacement agent prepared in Examples 1-3 are the largest, proving that the displacement agent has the best water plugging effect under high salt and high temperature conditions; in Example 4, due to the change in the molar ratio of acrylamide, N,N-methylenebisacrylamide, acrylic acid and poly(2-acrylamide-2-methyl-1-propanesulfonic acid), the amide group in the polyacrylamide molecule is greatly increased, the salt-resistant species are reduced, and the apparent viscosity, apparent viscosity after 30 days and expansion multiple of the displacement agent are reduced; in Example 5, due to the change in the molar ratio of acrylamide, N,N-methylenebisacrylamide, acrylic acid and poly(2-acrylamide-2-methyl-1-propanesulfonic acid), the proportion of sulfonic acid groups in the polyacrylamide molecule is increased. The ratio is increased, the strength of resistance to divalent ions is increased, but the salt resistance to monovalent metals is reduced, resulting in the apparent viscosity of the control and displacement agent, the apparent viscosity after 30 days and the expansion ratio are all reduced; Example 6 Due to the change in the mass ratio of bentonite, poly (2-acrylamide-2-methyl-1-propanesulfonic acid) and di-tert-butyl peroxide, the polymer content in the modified bentonite is relatively reduced, and the bentonite structure is relatively loose, so that the apparent viscosity of the control and displacement agent, the apparent viscosity after 30 days and the expansion ratio are all reduced; Comparative Example 1 uses polyacrylamide instead of modified polyacrylamide, which greatly reduces the apparent viscosity of the control and displacement agent, the apparent viscosity after 30 days and the expansion ratio; Comparative Example 2 uses bentonite instead of modified bentonite, resulting in the apparent viscosity of the control and displacement agent, the apparent viscosity after 30 days and the expansion ratio are all reduced.
[0107] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.
Claims
1. A high temperature and salt resistant gel flooding agent, characterized in that: The gel displacement agent comprises the following raw materials in parts by weight: 1-1.3 parts of modified polyacrylamide, 0.05-0.15 parts of composite cross-linking agent, 40-50 parts of modified bentonite, 0.5-1 parts of surfactant, 0.1-0.2 parts of stabilizer and 120-150 parts of water.
2. A high temperature and salt resistant gel flooding agent as claimed in claim 1, characterized in that: The modified polyacrylamide comprises the following preparation steps: (1) completely dissolving acrylamide, N,N-methylenebisacrylamide, acrylic acid, poly(2-acrylamide-2-methyl-1-propanesulfonic acid) and ammonium persulfate in water to form a solution A; (2) adding N,N,N,N-tetramethylethylenediamine to the solution A of step (1) to form a reaction solution B; (3) placing the reaction solution B in step (2) in a vacuum reactor at 60-70° C. for 8-10 hours to obtain a reaction solution C; (4) adding isopropanol to the reaction solution C of step (3) to generate a precipitate, which is filtered and dried to obtain the modified polyacryloyl.
3. A high temperature and salt resistant gel flooding agent as claimed in claim 2, characterized in that: The molar ratio of acrylamide, N,N-methylenebisacrylamide, acrylic acid and poly(2-acrylamide-2-methyl-1-propanesulfonic acid) is 1:(1-2):(1-3):(1-2).
4. A high temperature and salt resistant gel flooding agent as claimed in claim 2, characterized in that: The relative molecular weight of the modified polyacrylamide is ≥14 million.
5. The high temperature and salt resistant gel flooding agent according to claim 1, characterized in that: The modified bentonite comprises the following preparation steps: After bentonite, poly (2-acrylamide-2-methyl-1-propanesulfonic acid) and di-tert-butyl peroxide are mixed and stirred at 50-70° C. for 2-3 hours, the temperature is raised to 110-140° C. and stirred at high speed for 1-2 hours before discharging the material to obtain poly (2-acrylamide-2-methyl-1-propanesulfonic acid) modified bentonite.
6. A high temperature and salt resistant gel flooding agent as claimed in claim 5, characterized in that: The mass ratio of the bentonite, poly(2-acrylamide-2-methyl-1-propanesulfonic acid) and di-tert-butyl peroxide is 100:(12-20):(0.13-0.2).
7. The high temperature and salt resistant gel flooding agent according to claim 1, characterized in that: The composite cross-linking agent is resorcinol and benzaldehyde.
8. The high temperature and salt resistant gel flooding agent according to claim 1, characterized in that: The surfactant is one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium bromide, α-olefin sulfonate, and petroleum sulfonate.
9. The high temperature and salt resistant gel flooding agent according to claim 1, characterized in that: The stabilizer is one or more of sodium thiosulfate, thiourea, 2,4-dithiobiuret, semicarbazide, thiosemicarbazide, 1,4-phenylenebis(thiourea), and sodium polyphosphate.
10. A method for preparing a high temperature resistant and salt resistant gel flooding agent according to any one of claims 1 to 9, characterized in that: The steps include: S1, mixing water, modified bentonite, surfactant and modified polyacrylamide and stirring them uniformly to obtain a mixture A; S2, adding a stabilizer to the mixture A and stirring for 20-30 minutes, then adding a crosslinking enhancer and stirring evenly to obtain a mixture B; S3, adding a composite crosslinking agent to the mixture B in S2 and stirring for 30-40 minutes to obtain a mixture C; S4. Place the mixture C in S3 in a constant temperature box at 100-130° C. to react for 5-7 days to obtain a gel displacement agent.
Citation Information
Patent Citations
An integrated modulator and its preparation method and application
CN112708405B