Absorbable bone wax as well as preparation method and application thereof

By using the physical assembly technology of polyester and modified polysaccharide, absorbable bone wax with gradient degradation characteristics is prepared, which solves the problems of insufficient biocompatibility and adhesive properties of bone wax and achieves effective hemostasis of bone wounds. and healing.

CN118718073APending Publication Date: 2024-10-01WENZHOU INST UNIV OF CHINESE ACAD OF SCI

Patent Information

Application Number
CN202411215731.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Due to poor biodegradability, insufficient biocompatibility and insufficient adhesion properties of existing bone wax, complications such as delayed bone healing, foreign body reaction, tendon and nerve damage, and the degradation rate of absorbable materials are not suitable for bone wound repair.

Method used

Polyester, amino-terminated four-arm polyethylene glycol and modified polysaccharide are used to prepare absorbable bone wax with gradient degradation characteristics through physical assembly, including polycaprolactone, polyglycolic acid copolymer and modified polysaccharide. Sugar ensures good biocompatibility and stable bone wound bonding effect.

Benefits of technology

It achieves excellent hemostatic ability and ideal degradation in the rabbit iliac bone defect model, maintains the physical properties of traditional bone wax, and provides stable support on the bone wound surface and promotes healing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718073A_ABST
    Figure CN118718073A_ABST
Patent Text Reader

Abstract

The invention discloses absorbable bone wax as well as a preparation method and application thereof, and the absorbable bone wax with good biocompatibility, stable bone wound adhesion effect and gradient degradation characteristic is obtained by taking synthetic polyester, amino-terminated four-arm polyethylene glycol and modified polysaccharide as main raw materials through a physical assembly mode. The prepared bone wax keeps the physical characteristics and the use method of the traditional bone wax, and shows excellent hemostatic capacity and ideal degradation condition in a rabbit ilium defect model.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical materials, and in particular to absorbable bone wax and a preparation method and application thereof. Background Art

[0002] Bones are an important part of the human locomotor system and have a rich blood supply network. Bone injuries are often accompanied by the rupture of capillaries in the bones. Bleeding from such bone injuries usually presents as oozing blood. If the bleeding cannot be stopped in time and effectively, it will pose a threat to the patient's life safety. Bone wax is a filling agent used in orthopedics, thoracic surgery, neurosurgery, maxillofacial surgery and dental surgery to control bone bleeding. It is mainly composed of a mixture of beeswax and softeners such as vaseline, and has strong hydrophobicity. When in use, it can be easily rubbed and shaped after a slight warming in the hands, and filled into the bone oozing area to achieve physical occlusion and hemostasis. Despite this, bone wax may cause a variety of complications due to its poor biodegradability and biocompatibility, such as foreign body reaction and granuloma formation, affecting bone healing, severe tendon and nerve damage, intra-articular inflammatory response, surgical site infection and other problems. Therefore, in some cases, bone wax is not the best choice for hemostasis. When using it, its pros and cons must be weighed and alternative methods must be considered to ensure the safety and recovery of patients.

[0003] In recent years, absorbable bone hemostatic materials and integrated hemostatic-osteogenic materials have been widely studied and used for hemostasis and bone repair in orthopedic surgery. In 2005, Ceremed, an American company, launched Ostene, a cancellous bone wound hemostatic material based on alkylene oxide copolymers. The use of this material is similar to bone wax. After rubbing and shaping, it is stuffed into the bone wound surface. After use, it can be completely degraded in the body, ensuring that bone healing at the defect can start earlier. In addition, some domestic research teams have developed a variety of absorbable bone hemostatic materials based on a series of materials such as poloxamer, gelatin or collagen, polysaccharides, polylactic acid or polycaprolactone, and polyethylene glycol. On this basis, some bone hemostatic materials composited with bioactive glass, calcium apatite, and calcium sulfate have also been reported. After completing the hemostasis of the bone wound, the inorganic active components inside this type of material can promote cell proliferation and bone tissue production during the degradation process, thereby accelerating the repair of the bone defect wound. For example, a foreign research team has developed a material (BoneSeal) with waxy properties composed of hydroxyapatite and degradable polylactic acid. Its usage is similar to bone wax, and it can meet the hemostatic needs and has certain osteogenic properties. However, in summary, the materials currently under study still have the following problems: 1. Biocompatibility. For example, alkylene oxide copolymers and poloxamers have a destructive effect on cells, which may cause complications or delayed healing during use. 2. Adhesion properties. For example, although the mechanical properties of materials such as polylactic acid, polycaprolactone, and polyethylene glycol can reach the level of traditional bone wax, due to the properties and structure of the materials themselves, they cannot form a strong adhesion with the wound surface, which makes it easy to fall off during use and cannot play a hemostatic role. 3. Degradation rate. Most of the above-mentioned absorbable materials degrade too quickly, which makes it difficult to provide sufficient support during the healing process of bone wounds. If the degradation is too slow, it may affect the healing of the wound surface. Summary of the invention

[0004] In order to solve the shortcomings of the prior art, the present invention provides an absorbable bone wax and a preparation method and application thereof, which has good biocompatibility, a stable bone wound bonding effect and a gradient degradation characteristic.

[0005] The technical solution adopted by the present invention is: absorbable bone wax, which comprises polyester, amino-terminated four-arm polyethylene glycol 4ARM-PEG2000-NH2 and modified polysaccharide.

[0006] Specifically, the modified polysaccharide is one or more of active esterified hyaluronic acid HA5000-NHS or aldehyded dextran Dex5000-CHO.

[0007] Specifically, the polyester is polycaprolactone (PCL) and polycaprolactone / polyglycolic acid copolymer (PCL-PGA).

[0008] Specifically, the molecular weight Mw of the polyester is 800-4000.

[0009] Specifically, the absorbable bone wax comprises, by mass fraction, 25-45 parts of polycaprolactone, 15-35 parts of polycaprolactone / polyglycolic acid copolymer, 10-30 parts of 4ARM-PEG2000-NH2 and 10-20 parts of HA5000-NHS or Dex5000-CHO.

[0010] A method for preparing absorbable bone wax comprises the following steps: S1, synthesizing polyester: synthesizing polycaprolactone (PCL) and polycaprolactone / polyglycolic acid copolymer (PCL-PGA) of specific molecular weight by ring-opening polymerization: taking caprolactone, glycolic acid, a catalyst, and an initiator, adding them into a reaction device for sealed reaction; after the reaction is completed, cooling and taking out the product, vacuum drying, extracting, and vacuum drying the product to obtain polycaprolactone (PCL) and polycaprolactone / polyglycolic acid copolymer (PCL-PGA) with a molecular weight Mw of 800-4000; S2. Preparation of absorbable bone wax: At a temperature of 50-90°C, stir and disperse 25-45 parts of PCL, 15-35 parts of PCL-PGA, 10-30 parts of 4ARM-PEG2000-NH2 and 10-20 parts of HA5000-NHS or Dex5000-CHO in a stainless steel heating tank to allow the components to be fully mixed and assembled; then, pour the reaction system from the discharge port into a vacuum degassing device for degassing, and immediately pour the solution into a stainless steel mold while it is hot, let it stand and return to room temperature to obtain a molded material.

[0011] Specifically, the temperature is raised in step S1, and an inert gas such as N2 is introduced for protection before the reaction starts and throughout the reaction process.

[0012] An application of the absorbable bone wax in preparing bone injury hemostasis and repair materials.

[0013] The beneficial effects of the present invention are as follows: the present invention provides an absorbable bone wax and a preparation method and application thereof, using synthetic polyester, amino-terminated four-arm polyethylene glycol, and modified polysaccharide as main raw materials, and obtaining absorbable bone wax with good biocompatibility, stable bone wound adhesion effect, and gradient degradation characteristics through physical assembly. The prepared bone wax maintains the physical properties and usage methods of traditional bone wax, and exhibits excellent hemostatic ability and ideal degradation in a rabbit iliac bone defect model. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is the FT-IR spectrum of PCL.

[0015] Figure 2 The present invention is to evaluate the cytotoxicity of the absorbable bone wax prepared by the present invention.

[0016] Figure 3 It is an evaluation of the adhesion performance of the absorbable bone wax prepared by the present invention.

[0017] Figure 4 It is the degradation rate of the absorbable bone wax prepared by the present invention in the leaching under a specified time.

[0018] Figure 5 The present invention is a statistical data of the hemostasis success rate of the absorbable bone wax prepared in the present invention in a rabbit iliac bone volume defect bleeding model.

[0019] Figure 6 The graph shows the degradation of the absorbable bone wax prepared by the present invention at 2 weeks, 4 weeks and 8 weeks after the hemostasis of the rabbit iliac bone wound is completed. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1: Preparation of absorbable bone wax.

[0022] Synthetic polyester: Using a small high-pressure reactor, polycaprolactone (PCL) and polycaprolactone / polyglycolic acid copolymer (PCL-PGA) with specific molecular weight (Mw=800, 1500, 4000) are synthesized by ring-opening polymerization: in a glove box, a certain amount of caprolactone, glycolic acid, catalyst, and initiator are added to the reaction device in proportion and sealed; the device is placed in the reactor, the temperature is raised, and N2 and other inert gases are always introduced 1 h before the reaction and during the entire reaction process. After the reaction is completed, the temperature is lowered and the product is taken out, and the product is vacuum dried, extracted, and vacuum dried to obtain the final product. The molecular weight and chemical structure of the product are characterized, and by controlling the process parameters, PCL with a stable chemical structure and a specific molecular weight can be obtained.

[0023] Preparation of absorbable bone wax: At a specific temperature (50-90°C), 25-45 parts of PCL, 15-35 parts of PCL-PGA, 10-30 parts of 4ARM-PEG2000-NH2 and 10-20 parts of HA5000-NHS or Dex5000-CHO are stirred and dispersed in a stainless steel heating tank for 4 hours to allow the components to be fully mixed and assembled; then, the reaction system is poured from the discharge port into a vacuum degassing device for degassing, and the solution is immediately poured into a stainless steel mold while hot, allowed to stand and return to room temperature; the molded material is taken out of the mold and transferred to a cutting device for cutting; finally, the bone wax material is blister packed and irradiated for sterilization.

[0024] Experimental groups: Bone wax 1: 45 parts PCL, 15 parts PCL-PGA, 30 parts 4ARM-PEG2000-NH2, 10 parts HA5000-NHS Bone wax 2: 25 parts PCL, 25 parts PCL-PGA, 30 parts 4ARM-PEG2000-NH2 and 20 parts Dex5000-CHO Example 2: Chemical structure characterization of polyester The chemical structure of PCL was analyzed by Fourier transform infrared spectroscopy. Figure 1 As shown, the stretching vibration absorption peaks of -OH, -COC- and -C=O of PCL can be obtained from the spectrum.

[0025] Example 3: In vitro degradation Measure the initial weight of the sample (W0), soak the stent in 5 mL of sterile simulated body fluid solution, incubate in a 37°C incubator for 8 weeks, and weigh it after freeze-drying every week (W1). Evaluate the degradation performance of the stent based on the residual mass ratio (%) of the stent: Remaining mass ratio (%) = W1 / W0 × 100% The results are as follows Figure 4 As shown in the figure, the degradation rate of the two groups of bone waxes in the specified time in the leaching. Most of the bone waxes in the two groups were degraded in the first week, and then showed a slow degradation trend. Among them, the degradation ability of bone wax 2 was higher than that of bone wax 1. The mass of bone wax 2 was reduced to 15.8±1.7% at the 8th week, while the mass of bone wax 2 was reduced to 36.1±0.6% at the 8th week.

[0026] Example 4: Cytotoxicity In the leaching test, the sample extract was prepared (24 h). 3100 μl of osteoblast suspension was added to each well of a 96-well plate and incubated at 37°C for 24 h. Then, 100 μl of sample extract was used to replace the culture medium and incubated for 24 h and 48 h, respectively. Then, CCK-8 solution was added to each well for 2 h. Finally, the OD value at 450 nm was detected using a microplate reader (Varioskan LUX, ThermoFisher). The results are shown in Figure 2. Figure 2 As shown, the in vitro cell viability of osteoblasts after incubation with the material extract for 24 hours. All samples have good cell compatibility.

[0027] Example 5: Adhesion Performance The bovine cortical bone specimens were 80 × 10 × 2 mm cuboids. Before the test, the samples were kneaded and activated, and then placed in the middle of the bone blocks and a certain force was applied on one side to ensure that the other block was connected in a lap shear manner. After waiting for 10 minutes, the tensile adhesion strength test in the lap shear direction was carried out on a universal material testing machine, and the maximum stress before the bonded joint failed was recorded. The results are shown in Figure 2. Figure 3 As shown, in order to evaluate the potential application of bone wax in clinical situations, an in vitro experiment was conducted. The adhesion strength to cortical bone was measured by lap shear test using a universal testing machine. The experimental results showed that the two bone waxes in the experimental group had enhanced adhesion to the wound surface compared with the commercially available non-absorbable bone wax, which may be due to the formation of interaction forces including hydrogen bonds and chemical bonds between the components in bone wax 1 and 2 on the surface of cortical bone.

[0028] Example 6: In vivo animal experiment A circular defect with a diameter of 10 mm was made on the iliac bone of rabbits using a drill. A blank control group, a commercially available bone wax group, and an absorbable bone wax material group were set up and used on the defect wound surface. The effective hemostasis was recorded. The rabbits were killed 2 weeks, 4 weeks, and 8 weeks after the operation to observe the degradation of the material and the repair of the bone wound surface. Figure 5-6 As shown in the figure, all three types of bone wax can achieve effective hemostasis, but the commercially available non-absorbable bone wax showed no signs of degradation in 8 weeks, and the defective wound surface was not completely repaired. After 2 weeks of implantation, most of the bone wax 1 and 2 remained in the defective bone wound surface; after 4 weeks, most of the material had been degraded; after 8 weeks, both bone waxes had been completely degraded, and the defective bone tissue had been completely repaired.

[0029] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.

[0030] Technical personnel should note that although the present invention has been described according to the above specific implementation methods, the inventive concept of the present invention is not limited to this invention, and any modification using the inventive concept will be included in the scope of protection of this patent.

Claims

1. Absorbable bone wax, characterized in that: The absorbable bone wax comprises polyester, amino-terminated four-arm polyethylene glycol 4ARM-PEG2000-NH2 and modified polysaccharide.

2. The absorbable bone wax according to claim 1, characterized in that: The modified polysaccharide is one or more of active esterified hyaluronic acid HA5000-NHS or hydroformylation dextran Dex5000-CHO.

3. The absorbable bone wax according to claim 1, characterized in that: The polyesters are polycaprolactone (PCL) and polycaprolactone / polyglycolic acid copolymer (PCL-PGA).

4. The absorbable bone wax according to claim 1, characterized in that: The molecular weight Mw of the polyester is 800-4000.

5. The absorbable bone wax according to claim 3, characterized in that: The absorbable bone wax comprises, by mass fraction, 25-45 parts of polycaprolactone, 15-35 parts of polycaprolactone / polyglycolic acid copolymer, 10-30 parts of 4ARM-PEG2000-NH2 and 10-20 parts of HA5000-NHS or Dex5000-CHO.

6. A method for preparing absorbable bone wax according to claim 1, characterized in that: The following steps are involved: S1. Synthetic polyester: synthesize polycaprolactone (PCL) and polycaprolactone / polyglycolic acid copolymer (PCL-PGA) of specific molecular weight by ring-opening polymerization: take caprolactone, glycolic acid, catalyst, initiator, add them into the reaction device and seal them for reaction; after the reaction is completed, cool down and take out the product, vacuum dry, extract and vacuum dry the product to obtain polycaprolactone (PCL) and polycaprolactone / polyglycolic acid copolymer (PCL-PGA) with a molecular weight Mw of 800-4000; S2. Preparation of absorbable bone wax: At a temperature of 50-90°C, stir and disperse 25-45 parts of PCL, 15-35 parts of PCL-PGA, 10-30 parts of 4ARM-PEG2000-NH2 and 10-20 parts of HA5000-NHS or Dex5000-CHO in a stainless steel heating tank to allow the components to be fully mixed and assembled; then, pour the reaction system from the discharge port into a vacuum degassing device for degassing, and immediately pour the solution into a stainless steel mold while it is hot, let it stand and return to room temperature to obtain a molded material.

7. The preparation method according to claim 6, characterized in that: In the step S1, the temperature is raised, and an inert gas such as N2 is introduced for protection before the reaction starts and during the entire reaction process.

8. Use of the absorbable bone wax according to claim 1 in preparing hemostatic and repairing materials for bone injuries.

Citation Information

Patent Citations

  • Medical bleeding stopping and sealing material capable of being degraded and absorbed

    CN109646709A

  • Absorbable bone wax and preparation method thereof

    CN115645594A

  • Absorbable bone wax having function of promoting bone repair and preparation method thereof

    US20210162093A1

Cited By

  • Absorbable bone wax as well as preparation method and application thereof

    CN122786539A