Drug controlled-release gel stent based on 3D printing and preparation method of drug controlled-release gel stent

By using methacrylated silk fibroin and curcumin in drug-loaded stents, combined with DLP 3D printing technology, the problems of complexity and low precision in the preparation of drug-loaded stents are solved, and the preparation and production of high-precision, three-dimensional porous structures are achieved. Controlled drug release provides personalized treatment options.

CN118718092APending Publication Date: 2024-10-01SUZHOU UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410733394.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing preparation methods for drug-loaded stents are complex, making it difficult to achieve high-precision, customized design of complex structures and precise drug release. Common 3D printing technologies also suffer from problems such as poor structural self-support, low precision, and limited molding capabilities.

Method used

Using methacrylated silk fibroin (SilMA) as the main material, by adjusting the content of GMA and the concentration of curcumin, combined with DLP 3D printing technology, a high-precision, three-dimensional porous drug-controlled release gel stent was prepared and cured using light Technology enables on-demand loading and directional delivery of drugs.

Benefits of technology

It achieves the preparation of personalized, high-precision, three-dimensional porous drug-loaded scaffolds, improves the efficiency of drug release and the controllability of tissue repair, and provides an efficient treatment plan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718092A_ABST
    Figure CN118718092A_ABST
Patent Text Reader

Abstract

The invention discloses a drug controlled release gel scaffold based on 3D printing and a preparation method thereof, and the method comprises the following steps: adding a glycidyl methacrylate solution into a degummed silk fibroin solution, and carrying out a cross-linking reaction to obtain methacrylated silk fibroin; adding water to dissolve the methacrylated silk fibroin, adding curcumin, reacting, and adding a photoinitiator and a light blocking agent to obtain the drug-loaded bio-ink; and constructing a three-dimensional porous structure scaffold model, introducing the drug-loaded bio-ink into a DLP 3D printer, and printing to obtain the drug controlled release gel scaffold. According to the rapid DLP forming method of the drug-loaded bio-ink, the preparation process is simple, the tissue engineering scaffold and the therapeutic drug are effectively combined by adjusting the content of GMA, the concentration of SilMA and curcumin and DLP 3D printing parameters, and meanwhile, the rapid DLP forming method has good printing precision, formability and drug release capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of drug controlled-release gel scaffolds, and in particular to a drug controlled-release gel scaffold based on 3D printing and a preparation method thereof. Background Art

[0002] Three-dimensional printing (3DP), also known as additive manufacturing, is a rapid prototyping technology that has become increasingly popular in recent years. Compared with traditional scaffold preparation methods, 3D printing technology can perform high-resolution printing in the micron range. It has the ability to achieve precise manufacturing of geometric shapes and optimize scaffold structures. 3D printing uses software such as CAD, 3DMAX, and SolidWorks to design specific models and upload them to the printer, and then achieves the manufacture of three-dimensional structures by slicing and layer-by-layer printing. In recent years, 3D printing technology has developed rapidly in the field of biomedicine. 3D printing technology in the biomedical field is also called biological 3D printing technology (3D Bioprinting). Biological 3D printing is an interdisciplinary field that requires knowledge from developmental biology, stem cell science, chemistry, computer science, and materials science. Biological 3D printing technology has the characteristics of precise cell positioning, complex preparation structure, and high controllability. It has broad application prospects in the fields of tissue engineering, regenerative medicine, organ transplantation, drug release and high-throughput screening, and tumor research.

[0003] At present, the most widely used biological 3D printing technologies are mainly inkjet printing, extrusion printing and photocuring printing. Among them, photocuring 3D printing technology has developed rapidly due to its advantages such as high printing accuracy, smooth surface of printed objects, mild printing conditions, ability to print complex models, mature development and relatively low cost. Photocuring 3D printing technology is also called reductive photopolymerization technology, which refers to the preparation of three-dimensional structures by local photopolymerization and layer-by-layer curing of liquid photosensitive polymers. The use of focused photon beams to drive photosensitive biomaterials is the basis for the high resolution level that can be achieved by this bioprinting method. Photocuring 3D printing technology has great potential in the manufacture of biodegradable medical implants or devices due to its high accuracy and resolution, and may become an irreplaceable tool in personalized medicine. At present, photocuring 3D printing technology mainly includes stereolithography (SLA) technology, digital light processing (DLP) technology, continuous liquid interface production (CLIP) and other technologies. Among them, DLP is a local photopolymerization process based on the cross-section of the product, which mainly cures the liquid resin layer by layer through ultraviolet light UV projection, which can shorten the time of photocrosslinking of each layer. DLP bio 3D printer can print at 1mm per second 3 It provides fast printing time and a resolution of up to 1μm. It can be used to create small-sized, high-precision, and complex-structured tissue and organ models, and is increasingly used in the biomedical field.

[0004] Scaffolds are an important part of tissue engineering. The pore size and 3D spatial structure of scaffolds are key factors in cell adhesion, proliferation, differentiation and extracellular matrix (ECM) production in tissue engineering. Photocuring 3D printing technology can achieve precise porous structure design and reduce damage to cells. The pore size and distribution can be adjusted to provide a microenvironment for cell attachment, drug delivery and nutrient exchange. At the same time, the drug delivery system (DDS) constructed by photocuring 3D printing can achieve personalized drug loading and customized model preparation suitable for patients. The treatment formula can be formulated according to the needs of patients to achieve on-demand drug loading, directional delivery and long-term release. It has a wide range of applications in the development of personalized drugs and medical devices. Curcumin (Cur) is an active polyphenol compound extracted from the rhizome of turmeric. It has many ideal biological properties, such as promoting wound healing, anti-oxidation, anti-inflammatory, antibacterial, and anti-tumor. By using it as a therapeutic drug and combining it with an implantable porous scaffold, it can effectively improve the efficiency of tissue regeneration for tissue repair. However, curcumin itself has poor water solubility and poor oral bioavailability. Selecting a suitable encapsulation carrier and effectively transporting it to the required part of the human body to achieve drug release is the focus of current research.

[0005] Based on the principle of photocuring 3D printing technology, the ink material used in photocuring 3D printing technology must have photosensitive properties to complete the required structure molding through the photocrosslinking mechanism during printing, and can provide sufficient mechanical properties and biocompatibility after printing. Silk fibroin (SF) material is a natural polymer fibrous protein with excellent physical and chemical properties. Because of its good biocompatibility, biodegradability, adjustable mechanical properties, rich sources and easy processing, it has broad medical application prospects in tissue engineering, drug delivery, implantable degradable medical devices, etc. However, pure SF does not have photosensitive properties. When it is used in DLP printing, it needs to be modified. There are usually two ways to modify SF. One is to prepare ink by compounding photosensitive materials with SF materials. By mixing SF solution with materials with photosensitive groups and photoinitiators, and then crosslinking when exposed to light of appropriate wavelengths, an interpenetrating network structure with enhanced mechanical properties is formed. The other is to modify the functional groups of the SF material itself, by modifying the photosensitive functional groups onto the SF protein molecular chain, and using a photoinitiator to form a covalent bond between these functional groups, so that the SF-based ink has photosensitive properties and can be used for photocuring bioprinting. Patent CN113713179B provides a high comprehensive performance photocuring bio-3D printing composite hydrogel, which uses methacryloyl gelatin (GelMA), methacryloyl hyaluronic acid (HAMA) and methacryloyl silk protein (SilMA) as monomers for covalent cross-linking and curing to form a polymer gel, and by introducing double bonds on the basis of the material structure and using them in combination, the photosensitivity of the material is increased, and the modified material can form a covalent bond between molecules in the form of a monomer to produce a polymer network, so as to obtain a gel material with excellent comprehensive properties such as biocompatibility, formability, and mechanical properties and a fast cross-linking speed, and construct a tissue scaffold for the repair of nerve damage and the screening of nerve drugs. However, this invention uses more materials, the preparation and processing of the scaffold are more complicated, and it is not effectively combined with functional drugs. Patent CN117159801A provides a method for preparing a nanocomposite hydrogel scaffold for promoting bone tissue regeneration. This invention synthesizes methacryloyl gelatin (GelMA) and methacryloyl silk fibroin (SFMA) by modifying gelatin and silk fibroin, and then blends and disperses them with nanoparticles encapsulating osteoprotegerin (OPG) and stromal cell-derived factor-1 (SDF-1), and forms gel under light-induced conditions to obtain a functionalized bone tissue scaffold that can promote osteoblast migration and differentiation. However, the scaffold structure prepared by this method is simple and fixed, and it is difficult to achieve the preparation of a complex porous scaffold structure with a sustained release function.Patent CN112043870A relates to a method for preparing a 3D printed polyvinyl alcohol / calcium phosphate drug-loaded bone repair scaffold. The invention uses self-curing calcium phosphate powder as a matrix, and uses an acidic cross-linking system of polyvinyl alcohol and glutaraldehyde as a thickener to form a gel suitable for 3D printing stacking deposition, and adds glycerol to adjust the solution viscosity and the curing time of calcium phosphate. By directly adding bioactive drug powder or solution to the printing "ink", an implantable drug-loaded bone repair scaffold with hydroxyapatite as the main body is formed. However, the scaffold obtained by the stacking deposition type 3D printing molding method is difficult to form a three-dimensional structure with clear pores and a complex three-dimensional structure, while the connected pore size structure is more suitable for repair and regeneration of tissue defects and drug release.

[0006] Commonly used methods for preparing functional drug-loaded stents mainly include mold method, freeze-drying method, electrospinning process, laser sintering process, etc., and the stents prepared by these technologies are generally difficult to achieve personalized, complex three-dimensional structure molding and good biocompatibility at the same time. In addition, the drug loading method is generally achieved by microsphere encapsulation / adsorption or stent impregnation, which is relatively complicated. Compared with traditional processes, 3D printing can achieve better control of the properties of implant materials such as geometry, surface area, internal structure and release dynamics by precisely designing the microstructure, thereby achieving personalized treatment of tissue repair. However, there is currently a lack of design and research on the preparation of drug-loaded stents using photocuring, especially DLP 3D printing technology.

[0007] In summary, the drug-loaded stents prepared by conventional technologies generally have a complex preparation process, simple or fixed structures, and poor scalability and controllability. It is difficult to achieve customized design of high-precision, complex structural models for tissue repair and precise drug release. At the same time, the stent structures obtained by common extrusion or inkjet 3D printing technologies generally have poor self-support, low precision, limited molding capabilities, and often have problems such as clogging of the printing nozzle. Therefore, it is necessary to adopt a three-dimensional porous structure molding method with high precision that can achieve drug loading. It is necessary to develop and obtain the process parameters of a Cur-containing SF bio-ink with excellent printability, mechanical properties and biocompatibility for the preparation of drug-loaded three-dimensional structure stents. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a drug controlled-release gel scaffold based on 3D printing and a preparation method thereof. Methacrylylated silk fibroin (SilMA) is selected as the main material of the ink. By adjusting the content of GMA, the concentration of SilMA and curcumin, DLP 3D printing technology is used to achieve high-precision, three-dimensional porous drug-loaded scaffold light-curing 3D printing.

[0009] In order to solve the above technical problems, the first aspect of the present invention provides a method for preparing a drug controlled-release gel scaffold based on 3D printing, comprising the following steps:

[0010] S1, adding glycidyl methacrylate (GMA) solution to degummed silk fibroin (SF) solution for cross-linking reaction to obtain methacrylylated silk fibroin (SilMA);

[0011] S2, dissolving the methacrylylated silk fibroin in water, adding curcumin (Cur), and after the reaction, adding a photoinitiator and a light-blocking agent to obtain a drug-loaded bio-ink;

[0012] S3. Construct a three-dimensional porous structure scaffold model, introduce the drug-loaded bio-ink into a DLP 3D printer, and print the drug controlled-release gel scaffold.

[0013] The present invention selects natural material SF as the ink matrix material, and its good biocompatibility and physicochemical properties enable it to meet the design requirements as a tissue engineering material. Silk fibroin is modified by GMA to obtain methacrylylated silk fibroin, and curcumin, a photoinitiator, and a light-blocking agent are added to the methacrylylated silk fibroin aqueous solution to obtain a drug-loaded bio-ink. The drug-loading process is simple, and a high-precision, three-dimensional porous drug-loaded drug controlled-release gel scaffold is prepared by DLP 3D printing technology.

[0014] Furthermore, in S2, the mass of the curcumin is 0.5%-3% of the mass of water.

[0015] Furthermore, in S2, the mass of the methacrylylated silk fibroin is 20%-30% of the mass of water.

[0016] Furthermore, in S1, the concentration of the glycidyl methacrylate solution is 400 mM-750 mM, and the concentration of the silk fibroin solution is 20%-30% (w / v).

[0017] Furthermore, in S1, the volume ratio of the silk fibroin solution to the glycidyl methacrylate solution is 100:(6-10).

[0018] Furthermore, the solvent of the silk fibroin solution is 9.3 mol / L lithium bromide solution.

[0019] Furthermore, in S1, the cross-linking reaction is followed by dialyzation, and the mixture is frozen at -70°C to -85°C and freeze-dried for 2-5 days to obtain SilMA lyophilized powder, which has a more stable structure.

[0020] Furthermore, the dialysis uses a dialysis bag with a molecular weight cutoff of 12-14 kDa.

[0021] Furthermore, in S1, the conditions of the cross-linking reaction are: temperature of 55-65° C., time of 3-5 h, and rotation speed of 200-400 rpm.

[0022] Furthermore, in S2, the reaction conditions are: rotation speed 500-700 rpm, time 0.5-2 h.

[0023] Furthermore, the photoinitiator is one or more of phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (LAP), 2,2-diethoxyacetophenone (DEAP), riboflavin, photoinitiator 2959, etc., and the added amount of the photoinitiator is 0.2%-0.4% of the mass of water.

[0024] Furthermore, the photoresist is one or more of lemon yellow, methylene blue, carmine, etc., and the added amount of the photoresist is 0.04%-0.06% of the mass of water.

[0025] Furthermore, before S3, it also includes: placing the drug-loaded bio-ink in a debubbling machine for centrifugal debubbling, the debubbling parameters are: 1800-2200rpm, the time is 5-10min, and the structure of the printed scaffold after debubbling is more precise and clearer.

[0026] Furthermore, in S3, the light curing time of 3D printing is 55-65s.

[0027] The second aspect of the present invention provides a drug controlled-release gel scaffold based on 3D printing prepared by the preparation method described in the first aspect.

[0028] Beneficial effects of the present invention:

[0029] The present invention constructs a rapid DLP molding method for drug-loaded biological ink with a simple preparation process. Methacrylylated silk fibroin (SilMA) is selected as the main material of the ink. By adjusting the content of GMA, the concentrations of SilMA and curcumin, and the DLP 3D printing parameters, personalized high-precision, three-dimensional porous drug-loaded scaffolds can be photocured 3D printing, effectively combining tissue engineering scaffolds with therapeutic drugs. At the same time, it has good printing accuracy, molding properties and drug release ability, and can provide an efficient treatment plan for tissue repair and regeneration. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The full spectrum (a) and the regional enlarged spectrum (b) of the FTIR spectra of the comparative example 1 SF solution and the comparative example 2 SilMA bio-ink of the present invention;

[0031] Figure 2 1 is the H-NMR spectra of the SF solution of comparative example 1 and the SilMA bio-ink of comparative example 2 of the present invention;

[0032] Figure 3 It is the infrared spectra of curcumin of the present invention, comparative example 2, comparative example 3 and embodiment 1;

[0033] Figure 4 The graph is a graph showing the change in storage modulus G′ of SilMA inks with different parameters under UV irradiation conditions over time in Comparative Example 2, wherein (a) is SilMA-424mM ink with different SilMA concentrations, and (b) is 30% SilMA with different GMA contents;

[0034] Figure 5 This is a graph showing the relationship between the storage modulus G′ of the SilMA ink of comparative example 2 and the drug-loaded biological ink of example 1 under UV irradiation conditions and the time;

[0035] Figure 6 The moisture absorption curve (a) and swelling curve (b) of silMA hydrogels with different concentrations in Comparative Example 2;

[0036] Figure 7 The design model of the complex heterogeneous 3D structure printed by DLP of the silMA ink-printed stent in Comparative Example 2 and the actual photos of the corresponding printed stents: (a) rabbit stent; (b) liver unit stent; (c) ear stent; (d) minimal surface structure stent; (e) grid structure stent; (f) microporous cylindrical structure stent;

[0037] Figure 8 The following are photos of the SilMA-Cur drug-loaded stents with different pore size grid structures printed by DLP using the drug-loaded bio-ink in Example 1. The pore sizes from left to right are 0, 0.6 mm, and 0.8 mm, respectively: (a) front view of the stent loaded with 1% curcumin; (b) surface view of the stent loaded with 1% curcumin; (c) stereoscopic view of the stent loaded with 3% curcumin;

[0038] Fig. 9 Schematic diagram of the DLP-printed grid structure model of the 1% curcumin bio-ink in Example 1 and the corresponding ultra-depth optical microscope photos of the front and side of the SilMA-Cur drug-loaded stent: (a) non-porous block structure; (b) grid structure with a pore size of 0.6 mm; (c) grid structure with a pore size of 0.8 mm;

[0039] Fig.10 In comparative example 2, the GMA concentration is 705 mM, the silMA concentration is 30%, the UV exposure time is 30 s, the DLP printed grid structure model schematic diagram and the ultra-depth optical microscope photo of the printed 3D scaffold, wherein (a) a non-porous block structure; (b) a grid structure with a pore size of 0.6 mm; (c) a grid structure with a pore size of 0.8 mm;

[0040] Fig.11 The drug release curves of the curcumin-loaded hydrogel scaffold SilMA-Cur in Example 1: (a) the effect of the pore size of the grid structure loaded with 1% curcumin on drug release; (b) the effect of the pore size of the grid structure loaded with 3% curcumin on drug release. DETAILED DESCRIPTION

[0041] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0042] Comparative Example 1

[0043] (1) Raw silk degumming

[0044] Weigh 40g of raw silk, cut it into small pieces, measure 2L of deionized water and heat it in an induction cooker. After the water boils, add 10g of anhydrous sodium carbonate powder and raw silk, that is, dissolve the raw silk in a sodium carbonate solution with a concentration of 0.5% (w / v). Stir once every 10 minutes, boil for 30 minutes, take out the raw silk, put it in deionized water and scrub it 3-5 times to fully remove the sericin on the surface. Repeat the whole process three times to obtain the degummed silk. Tear the degummed silk into strips and place it in a 60℃ oven to fully dry it, then take it out for use.

[0045] (2) Preparation of silk fibroin (SF)

[0046] Take 20g of degummed silk after drying and dissolve it in 100mL of 9.3mol / L lithium bromide solution at a ratio of 1:5: first, measure two portions of 100mL lithium bromide solution and pour them into a beaker, seal it with aluminum foil, preheat it in an oven for 10 minutes, then gradually add the dried silk to the preheated lithium bromide solution in small amounts and multiple times, and stir it with a glass rod to make the silk fully contact, seal it with aluminum foil and put it in a 60℃ oven for 1h, stir it twice in the middle to make it fully dissolved. The obtained solution is cooled and filtered, then loaded into a dialysis bag with a molecular weight cutoff of 12-14kDa, and dialyzed with deionized water for three days; the obtained solution is centrifuged, then poured into a culture dish, first frozen in a refrigerator at -80℃ for 12 hours, and then placed in a freeze dryer for three days to obtain a freeze-dried SF sample.

[0047] (3) Take 1.5 g, 1.25 g, and 1 g of freeze-dried SF samples, add 5 mL of deionized water, stir with a glass rod to fully dissolve, then filter with a filter to eliminate bubbles on the surface, pour into a transparent sample bottle, and obtain SF solutions with concentrations (w / v) of 30%, 25%, and 20%. Store in a refrigerator at 4°C away from light.

[0048] Comparative Example 2

[0049] (1) Raw silk degumming

[0050] Weigh 40g of raw silk, cut it into small pieces, measure 2L of deionized water and heat it in an induction cooker. After the water boils, add 10g of anhydrous sodium carbonate powder and raw silk, that is, dissolve the raw silk in a sodium carbonate solution with a concentration of 0.5% (w / v). Stir once every 10 minutes, boil for 30 minutes, take out the raw silk, put it in deionized water and scrub it 3-5 times to fully remove the sericin on the surface. Repeat the whole process three times to obtain the degummed silk. Tear the degummed silk into strips and place it in a 60℃ oven to fully dry it, then take it out for use.

[0051] (2) Preparation of methacrylylated silk fibroin (SilMA)

[0052] Take 20g of degummed silk after drying and dissolve it in 100mL of 9.3mol / L lithium bromide solution in a ratio of 1:5: first measure two portions of 100mL of lithium bromide solution and pour them into a beaker, seal it with aluminum foil, and preheat it in an oven for 10 minutes. Then, gradually add the dried silk into the preheated lithium bromide solution in small amounts and several times, and stir with a glass rod to ensure full contact between the silk. After sealing it with aluminum foil, put it in an oven at 60℃ for 1h, and stir it twice in the middle to ensure full dissolution. In order to modify SF, after the silk was dissolved, 6 mL (424 mM) and 10 mL (705 mM) of glycidyl methacrylate (GMA) solution were added to two beakers for cross-linking, and a magnetic bar was placed, covered with aluminum foil, and the beaker was placed on a heated magnetic stirrer, set at 60 ° C, and the speed was 300 rpm. The reaction was carried out for 4 hours. The obtained solution was cooled and filtered, and then loaded into a dialysis bag with a molecular weight cutoff of 12-14 kDa, and dialyzed with deionized water for three days; the obtained solution was centrifuged, then poured into a culture dish, first frozen in a refrigerator at -80 ° C for 12 hours, and then placed in a freeze dryer for three days to obtain a freeze-dried SilMA sample. The concentration of added GMA was marked as SilMA-424mM and SilMA-705mM.

[0053] (3) Preparation of SilMA photocurable bio-ink

[0054] Take 1.5g, 1.25g, and 1g of freeze-dried SilMA-424mM and SilMA-705mM samples, add 5mL of deionized water, stir with a glass rod to fully dissolve, then filter with a filter to eliminate the bubbles on the surface, pour into a transparent sample bottle, and obtain SilMA solutions with concentrations (w / v) of 30%, 25%, and 20%. Then weigh 0.015g of photoinitiator LAP (0.3%) and 0.0025g of photoresist lemon yellow (0.05%), respectively, and add them to sample bottles containing different GMA contents and silMA concentrations, mix them thoroughly, and wrap the sample bottles with aluminum foil. Then place the sample bottles in a debubbler and confirm the weight, set the mode: speed 2000rpm, time 9min, and centrifuge to debubble. The debubbled photocurable bio-ink is obtained and placed in a 4°C refrigerator to store at low temperature away from light.

[0055] (4) constructing a three-dimensional porous structure scaffold model, introducing the drug-loaded bio-ink into a DLP 3D printer, and printing the drug controlled-release gel scaffold.

[0056] Comparative Example 3

[0057] (1) Raw silk degumming

[0058] Weigh 40g of raw silk, cut it into small pieces, measure 2L of deionized water and heat it in an induction cooker. After the water boils, add 10g of anhydrous sodium carbonate powder and raw silk, that is, dissolve the raw silk in a sodium carbonate solution with a concentration of 0.5% (w / v). Stir once every 10 minutes, boil for 30 minutes, take out the raw silk, put it in deionized water and scrub it 3-5 times to fully remove the sericin on the surface. Repeat the whole process three times to obtain the degummed silk. Tear the degummed silk into strips and place it in a 60℃ oven to fully dry it, then take it out for use.

[0059] (2) Preparation of methacrylylated silk fibroin (SilMA)

[0060] Take 20g of degummed silk after drying and dissolve it in 100mL of 9.3mol / L lithium bromide solution in a ratio of 1:5: first measure 100mL of lithium bromide solution and pour it into a beaker, seal it with aluminum foil, and preheat it in an oven for 10 minutes. Then, gradually add the dried silk into the preheated lithium bromide solution in small amounts and multiple times, and stir with a glass rod to ensure full contact between the silk. After sealing it with aluminum foil, put it in an oven at 60℃ for 1h, and stir it twice in the middle to ensure full dissolution. In order to modify SF, after the silk was dissolved, 10 mL (705 mM) of glycidyl methacrylate (GMA) solution was added to the beaker for cross-linking, and a magnetic bar was placed, covered with aluminum foil, and the beaker was placed on a heated magnetic stirrer, the temperature was set to 60°C, the speed was set to 300 rpm, and the reaction was carried out for 4 hours. The obtained solution was cooled and filtered, and then loaded into a dialysis bag with a molecular weight cutoff of 12-14 kDa, and dialyzed with deionized water for three days; the obtained solution was centrifuged and then poured into a culture dish, first frozen in a refrigerator at -80°C for 12 hours, and then placed in a freeze dryer for three days to obtain a freeze-dried SilMA sample.

[0061] (3) Take 1.5 g of the freeze-dried SilMA-705mM sample, add 5 mL of deionized water, stir with a glass rod to fully dissolve it, then filter with a filter to eliminate bubbles on the surface, pour into a transparent sample bottle, and obtain a SilMA solution with a concentration (w / v) of 30%. Then weigh 0.05 g (1%) of curcumin (Cur) drug, pour into the sample bottle, and freeze-dry to obtain SilMA-Cur foam.

[0062] Example 1

[0063] (1) Raw silk degumming

[0064] Weigh 40g of raw silk, cut it into small pieces, measure 2L of deionized water and heat it in an induction cooker. After the water boils, add 10g of anhydrous sodium carbonate powder and raw silk, that is, dissolve the raw silk in a sodium carbonate solution with a concentration of 0.5% (w / v). Stir once every 10 minutes, boil for 30 minutes, take out the raw silk, put it in deionized water and scrub it 3-5 times to fully remove the sericin on the surface. Repeat the whole process three times to obtain the degummed silk. Tear the degummed silk into strips and place it in a 60℃ oven to fully dry it, then take it out for use.

[0065] (2) Preparation of methacrylylated silk fibroin (SilMA)

[0066] Take 20g of degummed silk after drying and dissolve it in 100mL of 9.3mol / L lithium bromide solution in a ratio of 1:5: first measure 100mL of lithium bromide solution and pour it into a beaker, seal it with aluminum foil, and preheat it in an oven for 10 minutes. Then, gradually add the dried silk into the preheated lithium bromide solution in small amounts and multiple times, and stir with a glass rod to ensure full contact between the silk. After sealing it with aluminum foil, put it in an oven at 60℃ for 1h, and stir it twice in the middle to ensure full dissolution. In order to modify SF, after the silk was dissolved, 10 mL (705 mM) of glycidyl methacrylate (GMA) solution was added to the beaker for cross-linking, and a magnetic bar was placed, covered with aluminum foil, and the beaker was placed on a heated magnetic stirrer, the temperature was set to 60°C, the speed was set to 300 rpm, and the reaction was carried out for 4 hours. The obtained solution was cooled and filtered, and then loaded into a dialysis bag with a molecular weight cutoff of 12-14 kDa, and dialyzed with deionized water for three days; the obtained solution was centrifuged and then poured into a culture dish, first frozen in a refrigerator at -80°C for 12 hours, and then placed in a freeze dryer for three days to obtain a freeze-dried SilMA sample.

[0067] (3) Take 1.5g of the freeze-dried SilMA-705mM sample, add 5mL of deionized water, stir with a glass rod to fully dissolve it, then filter with a filter to eliminate the bubbles on the surface, pour into a transparent sample bottle, and obtain a SilMA solution with a concentration (w / v) of 30%. Then weigh 0.05g (1%) and 0.15g (3%) of curcumin (Cur) drugs, pour them into the sample bottles respectively, add a magnet, place them on a magnetic stirrer and stir for 1h, set the speed to 600rpm to fully mix them. Then weigh 0.015g of photoinitiator LAP (0.3%) and 0.0025g of photoresist lemon yellow (0.05%), add them to the sample bottle containing the SilMA-Cur mixed solution respectively, mix them thoroughly, and wrap the sample bottle with aluminum foil. Then place the sample bottle in a defoamer and confirm the weight, set the mode: speed 2000rpm, time 9min, and perform centrifugal defoaming. The degassed photocurable bio-ink was placed in a 4°C refrigerator and stored away from light.

[0068] (4) constructing a three-dimensional porous structure scaffold model, introducing the drug-loaded bio-ink into a DLP 3D printer, and printing the drug controlled-release gel scaffold.

[0069] Test Case

[0070] 1. Modification / grafting characterization

[0071] The SF solution of comparative example 1 and the SilMA photocurable bio-ink of comparative example 2 were subjected to infrared spectroscopy and H-NMR spectroscopy tests. The results are shown in Figure 1 and Figure 2 .

[0072] Depend on Figure 1 It can be seen that at 1286cm -1 The CHOH stretching of the alcohol group at 1168 and 947 cm-1 is attributed to the opening of the epoxy group of GMA when GMA modifies SF. -1 The peaks of CH2 and C=CH2 corresponding to the stretching vibrations of methacrylate vinyl groups gradually increased with the increase of GMA content, indicating that GMA successfully chemically modified SF.

[0073] refer to Figure 2 ,exist 1 In the H-NMR spectrum, compared with SF, the hydrogen spectrum of SilMA showed the methacrylic acid vinyl (double bond) signal of GMA at δ=6.05ppm and 5.6ppm, and the characteristic resonance of methyl (-CH3) in GMA appeared at δ=1.8ppm. In addition, the signal generated by hydrogen near the CN bond was found at δ=3.5-3.7ppm. These peaks also indicate that GMA has been successfully grafted onto the SF molecule.

[0074] 2. Chemical composition characterization

[0075] Curcumin, Comparative Example 2 (SilMA bio-ink), Comparative Example 3 (SilMA-Cur foam) and Example 1 (SilMA-Cur hydrogel printed scaffold) were subjected to infrared spectroscopy testing. The results are shown in Figure 3 In the spectrum of the freeze-dried foam sample obtained by mixing SilMA and curcumin, the characteristic peak of curcumin itself can be clearly seen, while in the spectrum of the curcumin-loaded hydrogel sample, the absorption peak of SilMA is basically displayed, and the peak value shifts to a low wavenumber, which indicates that hydrophobic interaction and hydrogen bonding may have occurred between SilMA and curcumin, and the loading of curcumin drug was achieved at the same time.

[0076] 3. UV rheological properties analysis

[0077] The rheological properties of the inks with different contents of GMA and SilMA in Comparative Example 2 and the inks with different contents of curcumin in Example 1 were analyzed. The results are shown in Figure 4 and Figure 5 During the DLP printing process, the SilMA ink is cross-linked by ultraviolet (UV) light to induce free radical polymerization, thereby promoting the transition of the ink from sol to gel.

[0078] refer to Figure 4, the storage modulus G' of the SilMA ink in comparative example 2 changes with time under UV irradiation conditions. It can be seen that the storage modulus of various SilMA inks increases rapidly after UV irradiation, and the ink undergoes elastic deformation, changing from liquid to solid, and the curing time is about 30s. At the same time, with the increase of GMA content and SilMA concentration, the storage modulus of the ink also increases. The SilMA (705mM) ink with a concentration of 30% can be cured quickly, and the storage modulus after curing can reach 26370Pa, indicating that the cross-linking degree between SF and GMA is higher and the photosensitivity is better.

[0079] Figure 5 The following is a graph showing the relationship between the storage modulus G′ and time of the SilMA-705mM ink in Comparative Example 2 and the drug-loaded bio-ink in Example 1 under ultraviolet light conditions. When the UV light source is turned on, the storage modulus of the ink loaded with different contents of curcumin drugs increases with the increase of light exposure time. Compared with the SilMA ink, the curing time of the ink after loading the curcumin drug increases. At the same time, the addition of too much curcumin will affect the cross-linked network inside the silMA and will also block the curing effect of the UV light source on the SilMA. The results show that the ink containing 1% curcumin has a good storage modulus and the curing time is about 60s.

[0080] 4. Characterization of moisture absorption / swelling properties

[0081] The moisture absorption and swelling performance of the SilMA-705mM hydrogels with different concentrations in Comparative Example 2 were analyzed. Figure 6 As the concentration of SilMA increases, its moisture absorption and swelling capacity decreases. The higher cross-linking density produces a tighter internal network structure, thereby hindering the massive penetration of water molecules. Therefore, the SilMA hydrogel with a concentration of 30% has relatively better moisture absorption and structural fidelity in the moist environment in vivo.

[0082] 5. Printability Characterization

[0083] The printability and shape fidelity of the SilMA ink and the drug-loaded SilMA ink prepared in Comparative Example 2 and Example 1 were studied. Figure 7 In comparative example 2, the 3D scaffold printed when the GMA concentration was 705 mM, the silMA concentration was 30%, and the UV exposure time was 30 s was as follows Figure 7 As shown, the various complex heterogeneous 3D structures printed are basically consistent with the pre-set model structure. The printed complex structures have clear textures and can reach the set height. The printed structures have clear contours and good stability, and have good complex structure and three-dimensional structure printing capabilities. Figure 8 and Fig. 9The actual digital photo and ultra-depth optical microscope photo of the porous grid structure hydrogel scaffold (silMA-Cur) loaded with curcumin drug printed by DLP in the drug-loaded bio-ink in Example 1, Fig.10 This is an ultra-depth optical microscope photo of the 3D scaffold printed by silMA in Comparative Example 2. Figure 8 It can be seen that the ink containing 1% curcumin has good printability, and the printed grid structure hydrogel scaffold is consistent with the set model in size and has good formability, while the formability of the ink containing 3% curcumin decreases.

[0084] Photographs taken from an ultra-deep-field optical microscope Fig. 9 and Fig.10 It can be seen that the hydrogel scaffold loaded with 1% curcumin can form a clearer and interconnected three-dimensional pore structure compared with the hydrogel scaffold without drug loading, and has better printability. However, the pore structure of the 3D scaffold printed by silMA in Comparative Example 2 is not clear. Fig.10 , which is a problem of clogging in porous structures; it shows that a small amount of curcumin drug molecules can be evenly dispersed into the internal pores of the hydrogel and make the structure of the hydrogel clearer and denser. It also proves that the bio-ink loaded with curcumin drugs has better printability than silMA ink.

[0085] 6. Characterization of drug release behavior of drug-eluting stents

[0086] The drug release performance of the curcumin-loaded hydrogel scaffold SilMA-Cur of Example 1 was analyzed to study the effects of different drug loadings and different pore sizes on the drug release behavior of the scaffold. The results are shown in Fig.11 The hydrogel scaffold containing curcumin has the effect of long-term slow release of drugs. Different drug-loaded scaffolds all show rapid release in the first 6 hours, and then gradually tend to stable release, and show an upward trend over time, indicating that the pore size of the scaffold and the drug loading of curcumin will not affect the drug release kinetics of curcumin. However, it will affect the release rate of the drug. As the pore size of the scaffold increases, the drug release effect increases, indicating that a higher surface area to volume ratio can increase the release rate of the drug.

[0087] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for preparing a drug controlled-release gel scaffold based on 3D printing, characterized in that: The steps include: S1, adding glycidyl methacrylate solution to silk fibroin solution to perform cross-linking reaction to obtain methacrylylated silk fibroin; S2, dissolving the methacrylylated silk fibroin in water and then adding curcumin, and after the reaction, adding a photoinitiator and a light-blocking agent to obtain a drug-loaded bio-ink; S3, constructing a three-dimensional network structure scaffold model, introducing the drug-loaded biological ink into a DLP 3D printer, and printing to obtain the drug controlled-release gel scaffold.

2. The method for preparing a drug controlled-release gel scaffold based on 3D printing according to claim 1, characterized in that: In S2, the mass of the curcumin is 0.5%-3% of the mass of water.

3. The method for preparing a drug controlled-release gel scaffold based on 3D printing according to claim 1, characterized in that: In S2, the mass of the methacrylylated silk fibroin is 20%-30% of the mass of water.

4. The method for preparing a drug controlled-release gel scaffold based on 3D printing according to claim 1, characterized in that: In S1, the concentration of the glycidyl methacrylate solution is 400 mM-750 mM, and the concentration of the silk fibroin solution is 20%-30% (w / v).

5. The method for preparing a drug controlled-release gel scaffold based on 3D printing according to claim 4, characterized in that: In S1, the volume ratio of the silk fibroin solution to the glycidyl methacrylate solution is 100:(6-10).

6. The method for preparing a drug controlled-release gel scaffold based on 3D printing according to claim 1, characterized in that: In S1, the cross-linking reaction is followed by dialyzation, and the mixture is frozen at -70°C to -85°C and then freeze-dried.

7. The method for preparing a drug controlled-release gel scaffold based on 3D printing according to claim 1, characterized in that: In S1, the conditions of the cross-linking reaction are: temperature of 55-65° C. and time of 3-5 h.

8. The method for preparing a drug controlled-release gel scaffold based on 3D printing according to claim 1, characterized in that: In S2, the reaction conditions are: rotation speed 500-700 rpm, time 0.5-2 h.

9. The method for preparing a drug controlled-release gel scaffold based on 3D printing according to claim 1, characterized in that: In S3, the light curing time of 3D printing is 55-65s.

10. A drug controlled-release gel scaffold based on 3D printing prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Hydrogel for improving photocuring 3D printing precision and application thereof

    CN119192614A

  • ROS-responsive broad-spectrum antibacterial 3D printing hydrogel loaded with yoghurt-derived exosome as well as preparation method and application of ROS-responsive broad-spectrum antibacterial 3D printing hydrogel

    CN121221840A