Preparation method and application of mechanical response bFGF (basic fibroblast growth factor) controlled-release hydrogel

By using alginate, sulfobetaine methacrylate and methacryloyl gelatin to prepare a mechanically responsive bFGF controlled-release hydrogel at the tympanic membrane perforation, the mechanical strength and function of traditional stent materials in a continuous mechanical vibration environment are solved. stability issues, achieving precise delivery and long-term controlled release of bFGF, promoting tympanic membrane healing and hearing recovery.

CN118718124APending Publication Date: 2024-10-01NINGBO MEDICAL CENT LIHUILI HOSPITACL +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410771502.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When dealing with tympanic membrane perforation, the existing technology is difficult to maintain the mechanical strength and functional stability of the stent material in a continuous mechanical vibration environment, resulting in delayed healing and hearing loss, and it is difficult for traditional drug-loaded stents to achieve precise delivery of growth factors and long-term durability. controlled release.

Method used

Using alginate, sulfobetaine methacrylate and methacryloyl gelatin as raw materials, bFGF-loaded microspheres were prepared through high-voltage electrostatic spraying technology and evenly dispersed in SBMA/GelMA hydrogel. Mechanically responsive bFGF controlled-release hydrogel was prepared by cross-linking method to achieve growth factor release and cell promotion under tympanic membrane vibration environment.

Benefits of technology

The hydrogel can stably release bFGF under mechanical vibration, promote cell migration and proliferation, improve the healing efficiency and hearing rehabilitation effect of tympanic membrane perforation, has good biocompatibility and tissue adhesion, and is suitable as a treatment for tympanic membrane perforation. Repair materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718124A_ABST
    Figure CN118718124A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of mechanical response bFGF (basic fibroblast growth factor) controlled-release hydrogel. The preparation method comprises the following steps: (1) preparing SA microspheres; (2) preparing an SBMA / GelMA hydrogel pre-polymerization solution; (3) uniformly dispersing the SA microspheres prepared in the step (1) into an SBMA / GelMA hydrogel prepolymer solution, sufficiently and uniformly mixing, and irradiating under an ultraviolet light source with the wavelength of 365 nm to obtain the mechanical response bFGF controlled-release hydrogel; the prepared bFGF controlled-release hydrogel can release growth factors in a mechanical response manner, has good tissue adhesion and biocompatibility, can adapt to a continuous mechanical vibration environment where a tympanic membrane is located when being used as a tympanic membrane perforation repair material, can maintain the mechanical strength, the functional stability and the tissue adhesion, and can be used for repairing the tympanic membrane perforation. In addition, the release of the bFGF can be controlled by utilizing the stimulation of mechanical vibration so as to promote cell migration and proliferation, so that a good treatment effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0002] The invention belongs to the field of biomedical materials, and in particular relates to a preparation method and application of a mechanically responsive bFGF controlled-release hydrogel. Background Art

[0003] Tympanic membrane perforation (TMP) is the most common otological disease in clinical practice, often caused by repeated middle ear infections, trauma, iatrogenic injuries, etc. Clinically, about 80% of acute TMP can heal on their own, but about 20% of patients cannot heal. When the perforation does not heal for more than 3 months, it will develop into chronic TMP. Chronic TMP can lead to hearing loss and recurrent otorrhea, and may even lead to complications within the temporal bone (such as labyrinthitis, peripheral facial palsy, Bezold abscess, etc.) and intracranial complications (such as epidural abscess, sigmoid sinus thrombophlebitis, meningitis, brain abscess, etc.). If intracranial infection occurs, it may even be life-threatening.

[0004] At present, tympanoplasty is the main treatment for chronic TMP. The operation aims to reconstruct the normal structure of the tympanic membrane and the acoustic vibration transmission mechanism. During the operation, autologous materials such as temporalis fascia, tragus cartilage, perichondrium and fat are used to repair the perforated tympanic membrane. However, the surgical repair method with autologous materials usually has the disadvantages of requiring general anesthesia, enlarging the incision for material collection, difficulty in reoperation, surgical anesthesia risk, and high cost. Growth factor therapy is a very promising treatment method. Since basic fibroblast growth factor (bFGF) can promote TMP healing by promoting cell proliferation, migration and vasodilation, gelatin sponge loaded with bFGF is currently commonly used in clinical treatment of TMP. However, bFGF has a short half-life, poor stability, and excessive doses can inhibit the synthesis of collagen in the fibrous layer. The above defects restrict its application in TMP. Therefore, it is urgent to construct a scaffold material that can load bFGF to achieve precise delivery and long-term controlled release of bFGF. However, traditional drug-loaded scaffolds often only consider their efficacy in a static state. In fact, the tympanic membrane is often under the continuous action of sound waves and sound pressure, and it deforms in real time and converts sound waves of different frequencies into vibrations. Since most scaffold materials are difficult to maintain their mechanical strength, functional stability and tissue adhesion in a continuous dynamic environment, it affects or delays the healing of perforations and may cause recurrent ear leakage and hearing loss. Therefore, in view of the continuous mechanical vibration environment of the tympanic membrane perforation, it is of great significance to develop a biomedical material that can mechanically respond to release growth factors and has good tissue adhesion and biocompatibility. Summary of the invention

[0005] The present invention aims to at least partially overcome the above-mentioned and / or other potential problems existing in the prior art: to provide a preparation method and application of a mechanically responsive bFGF controlled-release hydrogel. The bFGF controlled-release hydrogel prepared by the present invention can release growth factors in mechanical response and has good tissue adhesion and biocompatibility. When used as a repair material for tympanic membrane perforation, it can adapt to the continuous mechanical vibration environment of the tympanic membrane. It can not only maintain its mechanical strength, functional stability and tissue adhesion, but also use the stimulation of mechanical vibration to control the release of bFGF to promote cell migration and proliferation, thereby achieving a good therapeutic effect.

[0006] The present invention uses sodium alginate (SA), sulfobetaine methacrylate (SBMA) and gelatin methacrylate (GelMA) as raw materials, and adopts high-voltage electrostatic spraying technology to prepare SA microspheres loaded with bFGF, and then the microspheres are uniformly dispersed in the SBMA / GelMA hydrogel prepolymer solution by simple physical embedding, and the photocrosslinking method is used to form gel, thereby preparing a mechanical response bFGF controlled release hydrogel (SGM hydrogel) with rapid response ability. The hydrogel has good mechanical properties, tissue adhesion properties, and mechanical response properties. In addition, it also has good biocompatibility, can promote cell migration and proliferation by releasing biologically active bFGF, and vibration can promote bFGF release. The mechanical response hydrogel shows the potential for clinical treatment of TMP.

[0007] The technical solution of the present invention is as follows: A method for preparing a mechanically responsive bFGF controlled-release hydrogel comprises the following steps: 1) Preparation of SA microspheres: bFGF was dissolved in SA solution and bFGF-loaded SA microspheres were prepared by electrostatic spraying; 2) Preparation of SBMA / GelMA hydrogel prepolymer solution: GelMA was added to the SBMA solution, and then mixed with PEGDMA and Irgacure 2959 to obtain the SBMA / GelMA hydrogel prepolymer solution; 3) The SA microspheres prepared in step 1) are uniformly dispersed in the SBMA / GelMA hydrogel prepolymer solution, and after being fully mixed, they are irradiated under an ultraviolet light source with a wavelength of 365 nm to obtain a mechanically responsive bFGF controlled-release hydrogel.

[0008] Preferably, the GelMA is prepared by the following steps: gelatin is dissolved in a phosphate buffer solution at 50°C, methacrylic anhydride is added, phosphate buffer solution is added after 3 hours to terminate the reaction, dialyzed at 40°C, and freeze-dried to obtain GelMA.

[0009] The SA solution is an alginate solution. Specifically, the SA solution is a sodium alginate solution.

[0010] Preferably, in step 1), the concentration of sodium alginate in the sodium alginate solution is 1-2 wt %; and the content of bFGF in the sodium alginate solution is 0.2 ug / mL.

[0011] Preferably, the electrostatic spraying is a high-voltage electrostatic spraying technology with a voltage of 10-20 kV and an injection speed of 0.5-5 mL / h.

[0012] Preferably, the concentration of methacryloyl gelatin (GelMA) in the SBMA / GelMA hydrogel prepolymer solution is 2.5-10 wt %.

[0013] Preferably, the concentration of sulfobetaine methacrylate (SBMA) in the SBMA / GelMA hydrogel prepolymer solution is 1-1.5 g / ml.

[0014] Preferably, the concentration of polyethylene glycol dimethacrylate (PEGDMA) in the SBMA / GelMA hydrogel prepolymer solution is 0.10-0.15 wt %.

[0015] Preferably, the SBMA / GelMA hydrogel prepolymer solution contains 2-hydroxy-4 , -(2-Hydroxyethoxy)-2-methylphenylacetone (Irgacure 2959) concentration is 0.5-1.0wt%.

[0016] Preferably, in the mechanically responsive bFGF controlled-release hydrogel prepared in step 3), the content of SA microspheres is 2.5-10 wt %.

[0017] The present invention also provides an application of a mechanically responsive bFGF controlled-release hydrogel for preparing a tympanic membrane stent for treating tympanic membrane perforation, that is, as a medical material for preparing a repair material for tympanic membrane perforation.

[0018] Compared with the prior art, the beneficial effect of the present invention is that the hydrogel prepared by the present invention can promote the release of loaded bFGF in a mechanical response manner under continuous tympanic membrane vibration stimulation, thereby promoting TMP healing and hearing rehabilitation.

[0019] SA in the present invention is a natural polysaccharide extracted from brown algae, which has good stability and biocompatibility and is widely used in the fields of tissue engineering and regenerative medicine, including cell carriers, wound dressings and drug carriers. It is reported that the smaller the size of the smart hydrogel, the faster its response rate. Therefore, the present invention designs a hydrogel with a microsphere composite structure to achieve the purpose of improving the responsiveness of the smart hydrogel. The main advantage of using high-voltage electrostatic spraying technology is that the microsphere formation process occurs under relatively mild conditions, without the need for high temperature or the use of chemical cross-linking agents, does not affect the biological activity of growth factors, and is simple to operate and highly controllable. It can produce spherical, monodisperse and diameter-adjustable microspheres.

[0020] The SBMA self-polymer in the present invention, polysulfobetainemethacrylate (pSBMA), has excellent adhesion to tissues through ion-dipole and dipole-dipole interactions. Studies have shown that SBMA hydrogels can promote acute wound healing by promoting angiogenesis, reducing inflammatory responses, and regulating macrophage polarization. In addition, polySBMA also has the advantages of good biocompatibility and non-immunogenicity, making it a preferred alternative material for protein drug delivery systems. The above-mentioned methacryloyl gelatin (GelMA) is obtained by modifying gelatin by introducing methacrylate groups, and it has photocrosslinking properties. Adding GelMA to hydrogels can enhance the mechanical properties, bioactivity, and tissue affinity of hydrogels.

[0021] The hydrogel of the present invention has good mechanical properties and tissue adhesion properties. In particular, the release of bFGF can be controlled by mechanical vibration stimulation, and the vibration does not have a significant effect on the mechanical properties of the hydrogel, which indicates that the hydrogel has mechanical response properties. In vitro cytotoxicity experiments show that the hydrogel has good biocompatibility; immunofluorescence and scratch tests show that the bFGF-loaded hydrogel can release biologically active bFGF to promote cell migration and proliferation, and vibration can promote the release of bFGF.

[0022] The present invention uses sodium alginate microspheres as bFGF carriers, and simply physically embeds the smart microspheres so that they are embedded in the SBMA / GelMA hydrogel network structure, thereby preparing a hydrogel with rapid response capabilities, and proposing a "vibration-deformation-release" response mechanism. The hydrogel has good mechanical properties, tissue adhesion and biocompatibility, and is adapted to the unique dynamic mechanical environment of the tympanic membrane. It can release the loaded bFGF in a mechanical response manner under continuous tympanic membrane vibration stimulation. Therefore, the clinical method can control the drug release by giving auditory stimulation of different frequencies, accurately control the drug release dose, thereby meeting the drug needs of different healing stages, and promoting TMP healing and hearing rehabilitation. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 These are morphological images of the SA microspheres in Example 2, where (a) is an image of the SA microspheres; (b) is a polarizing microscope and scanning electron microscope image of the SA microspheres loaded with bFGF; and (c) is a fluorescence image of the SA microspheres loaded with FITC-bFGF.

[0024] Figure 2 The mechanical properties and adhesion performance curves of the hydrogel in Example 3, where (a) is the compressive stress-strain curve of the hydrogel; (b) is a picture of the hydrogel compressed to 80%; (c) is the tensile stress-strain curve of the hydrogel; and (d) is the adhesion-displacement curve of the hydrogel.

[0025] Figure 3 The release performance curve and fluorescence image of the hydrogel in Example 4, where (a) is the drug release curve of the hydrogel for 168 h; (b) is the fluorescence microscope image of the hydrogel containing SA microspheres (loaded with FITC-bFGF) vibrated at different frequencies for 2 h.

[0026] Figure 4 These are the compressive stress-strain curves of each group of hydrogels in Example 5 after vibration.

[0027] Figure 5 The biocompatibility comparison diagram of each group of hydrogels in Example 6; (a) is the relative proliferation rate of RS1 cells; (b) is the relative proliferation rate of HaCaT cells.

[0028] Figure 6 These are the phalloidin and DAPI staining images after the cells in Example 7 were co-cultured with the hydrogel extracts of each group for 5 days; (a) is RS1 cells; (b) is HaCaT cells.

[0029] Figure 7 The figures are the results of cell migration after culturing in the hydrogel extract for 24 h in Example 8, wherein (a) is a cell migration micrograph of RS1 cells; (b) is a cell migration micrograph of HaCaT cells; (c) is the cell migration rate of RS1 cells; and (d) is the cell migration rate of HaCaT cells. DETAILED DESCRIPTION

[0030] The present invention is further described in detail below with specific examples, but the present invention is not limited to the following specific examples.

[0031] Unless otherwise specified, the raw materials in the examples of this application are purchased through commercial channels. The mechanical response hydrogel in the examples is referred to as SGM. Each hydrogel comparison group is named SGxMy, where S is SBMA, G is GelMA, x is the mass percentage concentration of GelMA in the prepolymer solution, M is SA microspheres, and y is the mass percentage concentration of SA microspheres in the prepolymer solution; when y=0, SGxMy is also abbreviated as SGx.

[0032] Example 1 Preparation of mechanically responsive vibration SGM hydrogels: (1) Preparation of SA microspheres: Weigh 0.2 g of SA and add it to 10 mL of deionized water to obtain a 2% SA solution. High-voltage electrostatic spraying technology (height 10 cm, voltage 20 kV, injection rate 3 mL / h) was used to prepare SA microspheres.

[0033] (2) Preparation of GelMA: 1 g of gelatin was dissolved in 10 mL of phosphate buffer solution (PBS, 10 mm, pH 7.2 ± 0.2) at 50°C, and then 0.2 mL of methacrylic anhydride was slowly added. After 3 h, 40 mL of PBS was added to terminate the reaction. The mixture was dialyzed at 40°C for 3 days, and the product was collected by freeze drying to obtain GelMA.

[0034] (3) Preparation of SBMA / GelMA hydrogel prepolymer solution: 5 wt% GelMA was added to 2 mL of 1.4 g / mL SBMA solution, and then mixed with 2.8 mg PEGDMA and 15 mg Irgacure 2959.

[0035] (4) Preparation of SGM hydrogel: SA microspheres were evenly dispersed in the SBMA / GelMA hydrogel prepolymer solution, mixed thoroughly, injected into a glass mold, and irradiated under a 365 nm ultraviolet light source for 10 min to form SGM hydrogel.

[0036] Example 2 In an ice bath, fluorescein isothiocyanate (FITC) solution (5 mg / mL) was slowly added to bFGF solution (100 mg / mL) and reacted in a 4°C refrigerator away from light for 12 h. Hydroxylamine (final concentration of 0.15 M) was then added to terminate the reaction. The solution was then placed in a dialysis bag (molecular weight cutoff 12,000), dialyzed at 4°C, and finally collected by freeze-drying to obtain FITC-bFGF.

[0037] 0.2 μg / mL bFGF or FITC-bFGF was dissolved in SA solution, and SA microspheres loaded with bFGF or FITC-bFGF were prepared by the method described in Example 1. The morphology of the microspheres in a hydrated state was observed using a polarizing microscope, and the SA microspheres were dehydrated using an ethanol gradient dehydration method. After dehydration, the surface was sprayed with gold, and the microsphere morphology was observed using a scanning electron microscope. In addition, the fluorescence distribution of the SA microspheres loaded with FITC-bFGF was observed using an inverted fluorescence microscope.

[0038] Figure 1 is the morphology of SA microspheres, where Figure 1 (a) Image of SA microspheres prepared by electrostatic spraying process parameters using 2 wt% SA solution, voltage of 20 kV, and injection speed of 3 mL / h; Figure 1 (b) Polarized light microscope and scanning electron microscope images of bFGF-loaded SA microspheres; Figure 1 (c) is the fluorescence image of SA microspheres loaded with FITC-bFGF. Figure 1 It can be seen that SA microspheres with excellent shape and uniform size can be prepared by high-voltage electrostatic spraying technology. After the microspheres encapsulate bFGF, their size increases slightly, but the morphology of the microspheres is still relatively uniform. The bFGF-loaded microspheres prepared by the blending method have uniform fluorescence distribution without dark areas, indicating that bFGF is uniformly distributed in the microspheres, and no obvious phase separation occurs between bFGF and SA during the microsphere preparation process.

[0039] Example 3 The amount of SA microspheres added to the SBMA / GelMA hydrogel prepolymer solution in Example 2 was changed to form a control group, and 0 wt%, 2.5 wt%, 5 wt%, 7.5 wt%, and 10 wt% of SA microspheres were added, mixed thoroughly, and then photocrosslinked to form a gel. The corresponding hydrogel groups were named SG5, SG5M, and SG5M. 2.5 、SG5M5、SG5M 7.5 、SG5M 10 , the mechanical properties and adhesion properties of the above hydrogels were characterized using a universal testing machine.

[0040] (1) Mechanical properties characterization: The hydrogel samples were cut into 40 mm × 2 mm × 2 mm sizes and tested for tensile properties at a speed of 20 mm / min using a universal testing machine until they broke. In the compression test, the hydrogel samples were cut into cylindrical shapes with a diameter of 12 mm and a thickness of 5 mm and tested for compression properties at a speed of 0.5 mm / min using a universal testing machine at room temperature.

[0041] (2) Characterization of adhesion properties: The hydrogel was cut into 10 mm × 10 mm × 1 mm pieces and sandwiched between two titanium sheets wrapped with rabbit fascia. Before testing, a 100 g weight was placed on top of the hydrogel-fascia assembly for 1 h. The two ends of the assembly were fixed to a universal testing machine with clamps, and the assembly was pulled at a shear rate of 10 mm / min until it broke. The force-displacement curve of each sample was recorded.

[0042] result Figure 2 As shown, Figure 2 (a) is the compressive stress-strain curve of hydrogel; Figure 2 (b) is the morphology of the hydrogel compressed to 80%; Figure 2 (c) is the tensile stress-strain curve of hydrogel; Figure 2 (d) is the adhesion force-displacement curve of hydrogel.

[0043] Depend on Figure 2 (a) It can be seen that as the concentration of microspheres in the precursor solution increases from 0 wt% to 2.5 wt%, the compressive strength of the hydrogel increases from 8.5 MPa to 9.6 MPa. However, as the concentration of microspheres increases from 2.5 wt% to 5 wt%, the compressive strength of the hydrogel decreases significantly to 6.6 MPa. Figure 2 (b) It can be seen that when the loading concentration of microspheres exceeds 5 wt%, the resilience of the hydrogel decreases and cracks may appear when subjected to compression. Figure 2 (c) It can be seen that the tensile strength decreases from 175.2 kPa of SG5 to SG5M 10 46.7 kPa, however, the adhesive strength of the hydrogel only slightly decreased with the increase of microsphere content, e.g. Figure 2 (d) It can be seen that the temperature drops slightly from 52.8 kPa of SG5 to SG5M 10 of 45.1 kPa.

[0044] Therefore, based on the above compression, tensile and adhesion performance evaluations, SA microspheres with a concentration of 5 wt% are suitable for hydrogel preparation. SG5M5 hydrogel has good mechanical properties and adhesion properties. Based on the experimental results, its compressive strength, tensile strength, and adhesion strength are 6.6 MPa, 64.1 kPa, and 45.6 kPa, respectively.

[0045] Example 4 The SG5M5 hydrogel prepared in Example 3 was cut into a cylinder with a diameter of 19 mm and a thickness of 5 mm, placed on an electromagnetic vibration table, and 10 mL of PBS solution was added, followed by application of vibration forces of different frequencies (including 100 Hz, 500 Hz, 1000 Hz and 2000 Hz). In the control experiment, the same hydrogel was cultured in a PBS solution without any vibration. At each preset time point, 2 mL of sample solution containing released drugs was collected and then replaced with 2 mL of fresh PBS solution. The concentration of bFGF released by the hydrogel was determined by an enzyme-linked immunosorbent assay kit. Under different vibration conditions, the cumulative drug release of the hydrogel was calculated by the sum of the drug release within a certain period of time. In addition, the dispersion of the FITC-bFGF-loaded microspheres in the hydrogel was observed using a fluorescence microscope when the vibration force was applied or not.

[0046] Figure 3 The release performance comparison chart of hydrogels is shown in Figure 2. Figure 3 (a) Drug release curve of bFGF-loaded hydrogel for 168 h; Figure 3 (b) Fluorescence microscopy images of hydrogels containing SA microspheres (loaded with FITC-bFGF) vibrated at different frequencies for 2 h. The blue arrow indicates the release of bFGF.

[0047] from Figure 3 (a) It can be seen that SG5M5 hydrogel can make up for the deficiency of drug burst release of simple SA microspheres (indicated by M5 in the figure) and prolong the action time of bFGF at the perforated site. More importantly, SG5M5 hydrogel can control the release of hydrogel drugs through vibration stimulation. As the vibration frequency increases from 0 Hz to 1kHz, the cumulative release of bFGF gradually increases. However, when the vibration frequency increases from 1kHz to 2kHz, the cumulative release of bFGF in the hydrogel decreases.

[0048] from Figure 3 (b) It can be seen that under the action of vibration stress, the morphology of the microspheres changes and the internal fluorescence is unevenly distributed. The blue arrow in the figure shows that the green fluorescence accumulated outside the microspheres is then released into the hydrogel matrix and eventually diffuses into the surrounding environment. This "vibration-deformation-release" mechanism makes it possible to control the release of hydrogel drugs through vibration stimulation.

[0049] Example 5 The SG5M5 hydrogel was subjected to vibrations of different frequencies according to the method shown in Example 4. After vibration for 7 days, a compression test was performed again, and the test method was the same as that in Example 3.

[0050] Figure 4This is the compressive stress-strain curve of the hydrogel after vibration. It can be seen that the increase in vibration frequency has no significant effect on the compressive strength of the hydrogel, which indicates that the mechanical properties of the hydrogel are not affected by vibration.

[0051] Example 6 Rat skin fibroblasts (RS1) and human immortalized epidermal cell line (HaCaT) were used to evaluate the cell compatibility of hydrogels. The specific method is as follows: a certain amount of SG0 (prepared without adding GelMA to the prepolymer solution of Example 2), SG5 and SG5M5 hydrogels were placed in 5 mL of DMEM or MEM high-glucose complete medium, soaked at 37°C for 24 h, and the hydrogel extracts were labeled as SG0 group, SG5 group and SG5M5 group respectively. In addition, the SG5M5-1000 Hz group is a hydrogel extract obtained by vibrating SG5M5 hydrogel at a frequency of 1000 Hz for 1 day in DMEM or MEM complete medium under the same conditions. Then, the hydrogel extracts of each group were filtered with a 0.22 μm sterile filter. RS1 cells and HaCaT cells were cultured at 5×10 4 The cells were inoculated in a 24-well plate at a density of 100 μg / mL and 1 mL of DMEM or MEM high-glucose complete medium was added. The cells were cultured at 37°C and 5% CO2. After culturing for 24 h under the above conditions, the culture medium was discarded and replaced with 1 mL of the hydrogel extract of each group. The cells in the control group were cultured in DMEM or MEM high-glucose complete medium. After culturing for 24 h, the culture medium of each well was removed and the relative proliferation rate of the cells was determined using a cell counting kit-8 (CCK-8).

[0052] The results are as follows Figure 5 As shown, Figure 5 (a) Relative proliferation rate of RS1 cells; Figure 5 (b) is the relative proliferation rate of HaCaT cells. Figure 5 It can be seen that after 24 h of culture, the cell survival rate in each group was high, and the relative proliferation rate exceeded 80%, among which the relative proliferation rate of the SG0 group was the lowest, proving that each group of hydrogels had good cell compatibility. In addition, the introduction of GelMA can also improve the biocompatibility of the hydrogel.

[0053] Example 7 RS1 cells and HaCaT cells were cultured at 1.5 × 10 4 and 5×10 4The cells were inoculated at a density of 100 μg / mL in a 24-well plate loaded with cell slides. After culturing for 8 h at 37 °C and 5% CO2, the culture medium was replaced with hydrogel extracts (1 mL, 50 mg / mL) of the SG0, SG5, and SG5M5 groups, respectively. The cell culture conditions were the same as those in Example 6. After culturing for 5 days, the cells were stained with phalloidin and DAPI, and then the cell morphology was observed using a laser confocal microscope.

[0054] Figure 6 The pictures of phalloidin and DAPI staining after cells were co-cultured with hydrogel extracts from each group for 5 days. Figure 6 (a) RS1 cells; Figure 6 (b) is a HaCaT cell. Figure 6 It can be seen that the two types of cells aggregated into sheets, and the number of fluorescent cells in the SG5 group was greater than that in the SG0 group, indicating that the addition of GelMA increased the bioactivity of the hydrogel. At the same time, it can be seen that the number of cells in the vibration-released SG5M5-1000Hz group was greater than that in the SG5M5 group, and significantly greater than that in the experimental group without bFGF-loaded microspheres, proving that the SG5M5 hydrogel can release biologically active bFGF, thereby promoting cell proliferation. Under the action of mechanical vibration stress, the hydrogel can release more bFGF.

[0055] Example 8 RS1 cells and HaCaT cells were cultured at 5×10 4 and 8×10 4 The cells were plated at a density of 100 μg / mL and inoculated in a 24-well plate. DMEM or MEM high-glucose complete medium was added and cultured at 37 °C and 5% CO2. The next day, all cells were observed under a microscope. When the cell fusion reached more than 90%, a 10 μL sterile pipette tip was used to make scratches on the cell layer. The cells were then rinsed with sterile PBS to ensure that the detached cells were removed. Next, the extracts of the hydrogels of different groups in Example 6 extracted from DMEM or MEM high-glucose medium supplemented with 2% FBS were added to the wells. The cells in the control group were cultured in DMEM or MEM high-glucose medium containing 2% FBS. At each set time point (including 0 h, 12 h and 24 h), cell migration was observed under a microscope and photographed. The width of the scratch was measured using Image J software to calculate the cell migration rate.

[0056] Figure 7 is the migration result of cells cultured in hydrogel extract for 24 h, where Figure 7 (a) Microscopic image of cell migration of RS1 cells; Figure 7 (b) Microscopic image of cell migration of HaCaT cells; Figure 7 (c) Cell migration rate of RS1 cells; Figure 7(d) Cell migration rate of HaCaT cells.

[0057] Depend on Figure 7 It can be seen that after 24 h of culture, the scratches in the SG5M5 group and the SG5M5-1000Hz group were obviously closed by the migrating cells, while the number of migrating cells in the SG0 group, SG5 group and the control group was relatively small. In addition, the migration rate values ​​of the two cells co-cultured with the hydrogel extract of the SG5M5-1000Hz group were the highest. The above research results show that the SG5M5 hydrogel can release bioactive bFGF to promote the migration of epidermal cells, especially fibroblasts, and can promote the release of bFGF through mechanical vibration stress. Therefore, the mechanically responsive bFGF controlled-release hydrogel has the potential to promote tympanic membrane healing and clinical application.

[0058] The above are only examples of the features of the present invention and do not constitute any limitation on the protection scope of the present invention. Any technical solution formed by equivalent exchange or equivalent replacement falls within the protection scope of the present invention.

Claims

1. A method for preparing a mechanically responsive bFGF controlled-release hydrogel, characterized in that: The following steps are involved: 1) Preparation of SA microspheres: bFGF was dissolved in SA solution and bFGF-loaded SA microspheres were prepared by electrostatic spraying; 2) Preparation of SBMA / GelMA hydrogel prepolymer solution: GelMA was added to the SBMA solution, and then mixed with PEGDMA and Irgacure 2959 to obtain the SBMA / GelMA hydrogel prepolymer solution; 3) The SA microspheres prepared in step 1) are uniformly dispersed in the SBMA / GelMA hydrogel prepolymer solution, and after being fully mixed, they are irradiated under an ultraviolet light source with a wavelength of 365 nm to obtain a mechanically responsive bFGF controlled-release hydrogel.

2. The method for preparing the mechanically responsive bFGF controlled-release hydrogel according to claim 1, characterized in that: The GelMA is prepared by the following steps: gelatin is dissolved in a phosphate buffer solution at 50° C., methacrylic anhydride is added, phosphate buffer solution is added after 3 hours to terminate the reaction, dialyzed at 40° C., and freeze-dried to obtain GelMA.

3. The method for preparing the mechanically responsive bFGF controlled-release hydrogel according to claim 1, characterized in that: The SA solution is a sodium alginate solution.

4. The method for preparing the mechanically responsive bFGF controlled-release hydrogel according to claim 3, characterized in that: In step 1), the sodium alginate concentration in the sodium alginate solution is 1-2 wt %; the content of bFGF in the sodium alginate solution is 0.2 ug / mL.

5. The method for preparing the mechanical response bFGF controlled release hydrogel according to claim 1, characterized in that, The electrostatic spraying is specifically a high-voltage electrostatic spraying technology with a voltage of 10-20 kV and an injection speed of 0.5-5 mL / h.

6. The method for preparing the mechanically responsive bFGF controlled-release hydrogel according to claim 1, characterized in that: The concentration of GelMA in the SBMA / GelMA hydrogel prepolymer solution is 2.5-10 wt%.

7. The method for preparing the mechanically responsive bFGF controlled-release hydrogel according to claim 6, characterized in that: The concentration of SBMA in the SBMA / GelMA hydrogel prepolymer solution is 1-1.5 g / ml.

8. The method for preparing the mechanically responsive bFGF controlled-release hydrogel according to claim 7, characterized in that: The concentration of polyethylene glycol dimethacrylate PEGDMA in the SBMA / GelMA hydrogel prepolymer solution is 0.10-0.15wt%; the concentration of 2-hydroxy-4 , The concentration of -(2-hydroxyethoxy)-2-methylphenylacetone Irgacure 2959 is 0.5-1.0 wt %.

9. The method for preparing the mechanically responsive bFGF controlled-release hydrogel according to claim 8, characterized in that: In the mechanically responsive bFGF controlled-release hydrogel prepared in step 3), the content of the SA microspheres is 2.5-10 wt %.

10. Use of the mechanically responsive bFGF controlled-release hydrogel prepared according to any one of claims 1 to 9, characterized in that: Used to prepare tympanic membrane stents for treating tympanic membrane perforation.

Citation Information

Cited By

  • Alpha-lipoic acid liposome photo-thermal response type hydrogel coating capable of inhibiting scars and promoting wound healing as well as preparation method and application of alpha-lipoic acid liposome photo-thermal response type hydrogel coating

    CN120605367A