Degradation-controllable thermo-sensitive anti-adhesion hydrogel as well as preparation method and application thereof
The temperature-sensitive anti-adhesion hydrogel formed by combining sodium carboxymethylcellulose with polyether F127 solves the problem of postoperative abdominal adhesion, achieves stable stay in the abdominal cavity and effectively blocks fibrous adhesion, reducing the cost of surgery. Complexity and risk of complications.
Patent Information
- Application Number
- CN202410763059.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
AI Technical Summary
Postoperative abdominal adhesion is a common complication. Existing anti-adhesion materials are quickly removed from the abdominal cavity or are inconvenient to use, resulting in poor treatment effects, possible side effects, and increased surgical difficulty.
A temperature-sensitive anti-adhesion hydrogel with controllable degradation is used. By combining sodium carboxymethyl cellulose and polyether F127, a polymer network is formed, which uses temperature changes to gel in the body and form a protective layer on the wound surface. , prevent the excessive growth of fibrous tissue and inhibit the spread of inflammation.
The hydrogel can stay in the abdominal cavity for about 5 days, effectively blocks the formation of fibrous adhesions, has strong tissue adhesion, is suitable for laparoscopic surgery, is biodegradable, and reduces surgical complexity and risk of complications.
Smart Images

Figure HDA0004891606310000011 
Figure HDA0004891606310000012 
Figure HDA0004891606310000013
Abstract
Description
Technical Field
[0001] The present invention relates to the field of biomedical intelligent hydrogel materials, and in particular to a degradation-controllable temperature-sensitive anti-adhesion hydrogel and a preparation method and application thereof. Background Art
[0002] Postoperative abdominal adhesion is a common complication of general surgery and gynecological surgery. Although the environment and technology of surgical operations have been continuously improved in recent years, its incidence rate is still as high as 70-90%. Although most patients with abdominal adhesions will not have any symptoms, there are still about 20% of patients who will experience symptoms such as chronic abdominal pain, intestinal obstruction, and female infertility. Some even need a second operation to separate adhesions, which may lead to death in severe cases. Even for patients with asymptomatic abdominal adhesions, when another abdominal and pelvic surgery is required, the excessive fibrous tissue in the abdominal cavity will cause insufficient exposure of the surgical field and lesions, increase the difficulty of the operation, and prolong the operation time, which will inevitably lead to an increase in the incidence and mortality of other postoperative complications. The above problems will increase the pain and economic burden of patients and waste social medical resources, and a reasonable means of prevention and treatment is urgently needed.
[0003] Currently, a variety of measures have been applied to combat postoperative adhesions, including improved surgical techniques, drug therapy, and physical barriers. Drug therapy includes anticoagulants and anti-inflammatory drugs, such as heparin, streptokinase, dexamethasone, and other nonsteroidal anti-inflammatory drugs. Drug therapy is limited by rapid clearance in the peritoneal cavity and is prone to cause systemic side effects. Physical barriers include anti-adhesion fluids and solid sheets. Liquid barriers also stay too short due to rapid clearance in the peritoneal cavity, while solid sheets cannot be used conveniently during surgery or cannot completely cover the wound surface due to their volume and fixed shape.
[0004] Therefore, there is an urgent need to provide a new type of degradation-controllable temperature-sensitive anti-adhesion hydrogel and a preparation method thereof to solve the above problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a degradation-controllable temperature-sensitive anti-adhesion hydrogel and its preparation method and application. The preparation method is simple, the preparation conditions are easy to meet, no toxic or harmful chemical reagents are involved, no toxic or controversial by-products are produced, the product is stable and reliable, and can be prepared in large quantities.
[0006] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide a method for preparing a degradation-controllable temperature-sensitive anti-adhesion hydrogel, comprising the following steps:
[0007] Step 1: preparing sodium carboxymethyl cellulose solution;
[0008] Step 2: adding the sodium carboxymethyl cellulose solution prepared in step 1 to polyether F127 to prepare a degradation-controllable temperature-sensitive anti-adhesion hydrogel;
[0009] Step 3: The clarified liquid obtained in step 2 is sterilized by high temperature and high pressure sterilization.
[0010] In a preferred embodiment of the present invention, step 1 prepares the sodium carboxymethyl cellulose solution, comprising the following steps:
[0011] Sodium carboxymethyl cellulose is added to the solvent and vigorously stirred at 4 to 80° C. for 1 to 8 hours until the sodium carboxymethyl cellulose is completely dissolved, wherein the mass ratio of the sodium carboxymethyl cellulose to deionized water is 1:850 to 1:24.
[0012] Furthermore, the solvent is one or more of deionized water, physiological saline, buffer solution, simulated body fluid products, cell culture medium, human body fluid, and animal body fluid.
[0013] In a preferred embodiment of the present invention, step 2 of preparing a degradation-controllable temperature-sensitive anti-adhesion hydrogel comprises the following steps:
[0014] Add the sodium carboxymethyl cellulose solution prepared in step 1 to polyether F127 in a mass ratio of 3:1 to 17:3, and stir vigorously at room temperature for 0.5 to 2 hours until a white paste-like solid is formed. Place the substance in a 4°C refrigerator and let it stand for 8 to 48 hours until it becomes a foamy viscous liquid.
[0015] In a preferred embodiment of the present invention, step 3 sterilizes the clarified liquid obtained in step 2 with high temperature and high pressure, comprising the following steps:
[0016] The clarified liquid obtained in step 2 is placed in an autoclave for high pressure sterilization at 160-180°C for 2-4 hours, then taken out and stored in a refrigerator at 4°C.
[0017] In order to solve the above technical problems, another technical solution adopted by the present invention is: to provide a degradation-controllable thermosensitive anti-adhesion hydrogel prepared by the preparation method of the degradation-controllable thermosensitive anti-adhesion hydrogel as described in any of the above items.
[0018] In a preferred embodiment of the present invention, the hydrogel is a polymer network formed by physically cross-linking polyether F127 and carboxymethyl cellulose.
[0019] In a preferred embodiment of the present invention, the hydrogel is in a sol state at 4°C and can be injected into the postoperative wound surface by a syringe; and is in a gel state at 37°C and can cover the wound surface without flowing.
[0020] In order to solve the above technical problems, the third technical solution adopted by the present invention is: to provide a degradation-controlled thermosensitive anti-adhesion hydrogel as described in any of the above items for use in tissue repair of postoperative abdominal adhesions, postoperative pelvic adhesions and other wounds caused by surgical trauma.
[0021] Hydrogel is a polymer material widely used in the biomedical field. Its characteristic is that it can absorb a large amount of water in aqueous solution and self-assemble into a three-dimensional network structure. Hydrogel materials have a high water content and are similar to human tissues. Some specific hydrogel materials have good biocompatibility, blood compatibility, biodegradability, tissue adhesion and other characteristics. They can be safely used in vivo and in vitro, and have broad prospects in anti-adhesion and tissue repair.
[0022] Polyether F127 is a triblock copolymer composed of polyoxyethylene and polyoxypropylene, in which the difference in hydrophilic and hydrophobic properties of polyoxyethylene and polyoxypropylene makes its aqueous solution have the performance of responding to temperature, can flow freely at low temperature, and gel when close to human body temperature. The material has good biocompatibility and blood compatibility, and its aqueous solution already has commercial medical products. However, the network arrangement of pure F127 hydrogel is regular and linear, and it is very easy to degrade in the environment composed of aqueous solution, and the adhesion strength to tissue is not high, which limits its further application. Sodium carboxymethyl cellulose is a carboxymethyl derivative of cellulose. It is widely used as a thickener in the food and pharmaceutical industries. As an edible material, it has excellent biocompatibility. Under certain conditions, it can simulate the extracellular matrix environment, promote cell growth and wound recovery, and at the same time resist fibroblast and blood cell adhesion, prevent fibroblasts and inflammation-related immune cells from entering the gel, and inhibit the spread of inflammation and excessive growth of fibrous tissue. There are a large number of hydrogen bonds in its gel network, which is hydrophilic and rehydrating, and can accommodate a large number of water molecules.
[0023] Adding sodium carboxymethyl cellulose to the polyether F127 network can significantly enhance the non-covalent cross-linking rate between F127 molecules, and form a carboxymethyl cellulose protective layer on the surface after contacting water, preventing the aqueous solution from further contacting the F127 network and prolonging the degradation time of the hydrogel. The degradation rate and adhesion strength to the tissue can be adjusted by changing the hydrogel component ratio. In addition, the protective layer can absorb inflammatory exudate, provide an environment that simulates the extracellular matrix for the wound surface, further increase the biocompatibility of the hydrogel, and have the functions of anti-inflammatory and promoting wound recovery.
[0024] Compared with existing or researched anti-adhesion materials, this material has the following characteristics: no complex chemical modification is involved in the preparation process, and no toxic or harmful reagents are used in the whole process; the obtained hydrogel material can be sterilized and disinfected at high temperature; the components of the hydrogel form a gel through physical cross-linking of the polymer network, and reversible gelation can occur under the influence of temperature; no cross-linking agent is required to form gel, no reaction will occur in the body cavity, and it will not be affected by the rapid clearance of the abdominal cavity. The degradation rate of the hydrogel in the body is slow and adjustable; it has strong and adjustable tissue adhesion, and is not easy to fall off from the wound surface after gelation.
[0025] The beneficial effects of the present invention are as follows: compared with existing postoperative anti-adhesion barriers, drugs, etc., the hydrogel material will not be affected by the rapid clearance of the abdominal cavity, can stay on the wound surface in the abdominal cavity for about 5 days, and effectively prevent the formation of fibrous adhesion; it can be injected and used, and is suitable for laparoscopic surgery; it can quickly respond to changes in external temperature, gel in situ, has strong tissue adhesion, and perfectly fits the surface of various organs without the need for additional suturing and fixation; it is biodegradable and does not need to be removed during a secondary operation; the carboxymethyl cellulose protective layer formed on the surface of the hydrogel can maintain the stability of the gel, provide an extracellular matrix-like environment for the wound, promote wound healing, and at the same time resist the adhesion of fibroblasts and blood cells, prevent them from entering the interior of the gel, and inhibit the spread of inflammation and excessive growth of fibrous tissue. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The invention discloses the gelation state and temperature sensitivity of the thermosensitive anti-adhesion hydrogel with controllable degradation after being prepared with different solvents (deionized water, physiological saline, phosphate buffer, DMEM culture medium), and the injectability of the hydrogel prepared with deionized water;
[0027] Figure 2 is the variation curve of the relationship between the adhesion strength and displacement of the hydrogel between two pieces of pig skin;
[0028] Figure 3 It is the in vitro degradation curve of the hydrogel and the comparison chart of the degradation test effect with that of the pure polyether F127 hydrogel;
[0029] Figure 4 This is a comparison of the effects of the extract and diluted solution of the hydrogel on the viability of mouse-derived L929 cells and human colon epithelial NCM460 cells;
[0030] Figure 5 This is the application of the hydrogel in a rat postoperative abdominal adhesion model and the anti-adhesion effect diagram;
[0031] Figure 6 This is a Masson section of the intestinal wall and abdominal wall of a rat model seven days after application of the hydrogel;
[0032] Figure 7is the expression level of α-SMA in the intestinal wall and abdominal wall of the rat model seven days after application of the hydrogel. DETAILED DESCRIPTION
[0033] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0034] Embodiments of the present invention include:
[0035] Example 1: Preparation of hydrogel
[0036] A method for preparing a degradation-controllable temperature-sensitive anti-adhesion hydrogel comprises the following steps:
[0037] Step 1: Add sodium carboxymethyl cellulose into deionized water and stir vigorously at 60° C. until the sodium carboxymethyl cellulose is completely dissolved, wherein the mass ratio of sodium carboxymethyl cellulose to deionized water is 1:39.
[0038] Step 2: Add the obtained sodium carboxymethyl cellulose solution to polyether F127 in a mass ratio of 4:1. Stir vigorously at room temperature until a white paste solid is formed, and place the substance in a 4°C refrigerator for more than 12 hours until it becomes a clear, foamy, viscous liquid.
[0039] Step 3: The obtained clear liquid was placed in an autoclave for autoclaving at 180° C. for 4 hours, taken out, and stored in a refrigerator at 4° C. The hydrogel was labeled as hydrogel 1.
[0040] Referring to steps 1 to 3, hydrogel 2 and hydrogel 3 were prepared. The characteristic of hydrogel 2 is that the mass ratio of sodium carboxymethyl cellulose and deionized water in step 1 is adjusted to 1:79; the characteristic of hydrogel 3 is that the mass ratio of sodium carboxymethyl cellulose and deionized water in step 1 is adjusted to 0:80.
[0041] Meanwhile, referring to steps 1 to 3, hydrogel 1a, hydrogel 1b and hydrogel 1c were prepared. The hydrogel 1a is characterized in that the deionized water solvent in step 1 is replaced with physiological saline; the hydrogel 1b is characterized in that the deionized water solvent in step 1 is replaced with phosphate buffer; the hydrogel 1c is characterized in that the deionized water solvent in step 1 is replaced with DMEM culture medium.
[0042] In the preparation method of the hydrogel, the raw materials are easy to obtain, the preparation conditions are simple, the reaction is mild, no toxic or harmful chemicals are used, the product is stable, resistant to high temperature, severe shaking, and long-term storage, and does not contain toxic or controversial ingredients.
[0043] Example 2: Temperature sensitivity test
[0044] 5-7 ml of the hydrogel 1 prepared in Example 1 was placed in a centrifuge tube, 100 μl of 0.52 mg / ml rhodamine B reagent was added for color development, and the centrifuge tube was inverted or flipped at 4° C. and 37° C. After the gel in the tube was cooled, the hydrogel was extracted with a syringe and injected into a beaker containing 37° C. deionized water.
[0045] Similarly, 5-7 ml of hydrogel 1a, hydrogel 1b and hydrogel 1c prepared in Example 1 were placed in centrifuge tubes, and the centrifuge tubes were inverted or turned over at 4° C. and 37° C., respectively.
[0046] like Figure 1 As shown, hydrogel 1 and its derivatives hydrogel 1a, hydrogel 1b and hydrogel 1c can flow freely at 4°C, but form a gel at 37°C and do not flow with the inversion of the vial; the cooled hydrogel 1 can be injected through a syringe to form a gel in deionized water at 37°C.
[0047] This experiment verifies that the hydrogel is thermosensitive and can be liquid at low temperatures and gel at human body temperature, allowing it to be injected and used in various laparoscopic surgeries and to gel in situ on the tissue surface without the use of cross-linking agents or chemical reactions.
[0048] Example 3: Adhesion Strength Test
[0049] Take fresh pigskin, rinse it in phosphate buffer, wipe off the surface liquid, cut it into 3.0×3.0 cm square pieces, and fix it on the fixture of a special universal testing machine. Add 0.3 ml of the hydrogel 1 prepared in Example 1 to the surface of two pigskins, evenly apply it between the two pigskins, and incubate it at 37°C for 10 minutes to form a gel. Fix the fixture on the universal testing machine and set the displacement speed to 10 mm / min.
[0050] Similarly, 0.3 ml of hydrogel 3 prepared in Example 1 was added to the surface of the other two pigskins, evenly spread between the two pigskins, and incubated at 37° C. for 10 minutes to form a gel. The fixture was fixed on a universal testing machine, and the displacement speed was set to 10 mm / min. The adhesion strength of hydrogel 1 and hydrogel 3 was compared.
[0051] like Figure 2 As shown, the maximum adhesion strength of hydrogel 1 reached 7.67 kPa, which was much higher than the 1.37 kPa of hydrogel 3, proving that the adhesion of the hydrogel prepared by this method was improved compared with that of pure F127 hydrogel.
[0052] This experiment verifies that the hydrogel has the advantage of controllable tissue adhesion, and its maximum adhesion strength far exceeds that of pure F127 hydrogel. It also effectively overcomes the problem of poor mechanical strength of pure polyether F127 hydrogel, and can ensure a firm bond between the material and the wound surface without falling off from the wound surface prematurely.
[0053] Example 4: Degradability Test
[0054] Take 1 ml of hydrogel 1, hydrogel 2, and hydrogel 3 prepared in Example 1 and place them at the bottom of a centrifuge tube. Incubate at 37°C for 2 hours to form a gel, and weigh and record the initial weight of the hydrogel. Use a phosphate buffer solution with rhodamine B to soak the formed hydrogel at 37°C. Discard the liquid above the centrifuge tube every 24 hours, weigh and record the remaining weight of the hydrogel, and re-add phosphate buffer to continue degradation after completion. Repeat the above steps until the above groups of hydrogels are completely degraded. According to the obtained weight record, draw a degradation rate-degradation time change curve.
[0055] like Figure 3 As shown in the figure, on the sixth day, it can be seen that hydrogel 3 (pure polyether F127 hydrogel) has been completely degraded, while hydrogel 1 prepared by the present invention still remains. The degradation rate-degradation time change curve shows that hydrogel 1 can stably exist in the buffer solution for about 11 days, hydrogel 2 can stably exist in the buffer solution for about 7 days, and hydrogel 3 can only exist in the buffer solution for about 5 days. The above hydrogels can all degrade by themselves, meeting the needs of anti-postoperative adhesion.
[0056] This experiment verifies that the degradation rate of the hydrogel is controllable, which effectively overcomes the problem of excessive degradation of pure polyether F127 hydrogel, and ensures that the hydrogel material plays a role in isolating the wound surface during the critical period of postoperative abdominal adhesion formation.
[0057] Example 5: Cell viability comparison test
[0058] The hydrogel extract and hydrogel dilution described in this example were prepared according to the following method:
[0059] Take out 1 ml of the prepared hydrogel 1 solution from the refrigerator, add it to the bottom of the test tube, seal it and place it in a 37°C incubator for 2 hours to gel. After gelation, add DMEM culture medium to the test tube, soak the gel at 37°C for 24 hours, shake it well and pour out the supernatant to prepare the hydrogel extract.
[0060] The prepared hydrogel 1 was freeze-dried, and the hydrogel powder was added to DMEM culture medium at a mass ratio of 1:500 to prepare a hydrogel diluent.
[0061] Mouse fibroblasts L929 and human colon epithelial cells NCM460 were inoculated into 96-well cell culture plates and cultured for 24 hours at 37°C, 5% CO2, and 90% humidity to allow them to adhere to the wall. The original culture medium was removed, and 200 μl of DMEM culture medium, hydrogel extract, and hydrogel dilution were added to the wells of different rows of cells, and cultured again under the same conditions for 48 hours. 10 μl of Cell Counting Kit-8 solution was added to each well, and cultured under the same conditions for 3 hours. The absorbance of each well was measured at 450 nm using an ELISA reader.
[0062] like Figure 4 As shown, compared with the simple DMEM culture medium environment, the cell viability obtained by culturing in the hydrogel extract and hydrogel dilution solution was significantly improved.
[0063] Example 6: Application of hydrogel in rat postoperative abdominal adhesion model and anti-adhesion test
[0064] The rat postoperative abdominal adhesion model in this embodiment was constructed according to the following method:
[0065] Seven-week-old male SD rats were placed in a laboratory environment and fed freely for one week. The rats were fasted and given intramuscular injection of sodium ceftriaxone for infection the night before surgery. The rats were shaved and skinned. The rats were anesthetized with isoflurane gas anesthesia (4% concentration for induction and 2% concentration for maintenance) using a small animal anesthesia machine. Iodine was used for disinfection and draping. The skin and abdominal wall were cut along the midline of the abdomen to fully expose the cecum and the corresponding lateral abdominal wall. The surface of the cecum was abraded with a sterile brush until there was punctate bleeding; the peritoneum and superficial muscle layer on the surface of the abdominal wall were removed with ophthalmic scissors. After the blood on the wound was wiped with gauze, the mesentery was sutured to the abdominal wall with 5-0 silk sutures to make the two wound surfaces meet. The positive control group used 1 ml of normal saline to rinse the wound, the sham operation group did not cause damage to the intestinal wall and abdominal wall, and the hydrogel group used 1 ml of hydrogel 1 to be injected into the wound to form a gel. The abdominal wall and skin were sutured layer by layer. The rats resumed free diet after surgery.
[0066] The rats were divided into control group, sham operation group and hydrogel group according to the modeling method. On the seventh day after surgery, laparotomy was performed to explore the intra-abdominal adhesion and wound recovery, and the adhesion degree was scored. The specific scoring rules are as follows:
[0067] 0 points, no adhesion; 1 point, 1 thin adhesion that can be separated by blunt separation; 2 points, more than 1 thin adhesion that can be separated by blunt separation; 3 points, 1 thick strong adhesion that cannot be separated by blunt separation at the injury site; 4 points, more than one strong adhesion at the injury site; 5 points, extensive adhesions with angiogenesis in the fibrous tissue.
[0068] Seven days after surgery, after gross evaluation, intestinal wall-abdominal wall adhesion samples were collected, one part was fixed in 4% paraformaldehyde for pathological analysis, and the other part was stored in a -80°C refrigerator for subsequent molecular biological analysis.
[0069] Tissue samples fixed in paraformaldehyde were taken, dehydrated, de-alcoholized, paraffin-embedded, sliced, mounted, deparaffinized, stained, etc., to make pathological sections for observation and analysis under a microscope.
[0070] Take frozen fresh tissue, perform tissue grinding and lysis, protein extraction and denaturation, protein electrophoresis, membrane transfer, immunoreaction, chemiluminescence, etc., obtain Western-blot experimental bands, ImageJ TM The grayscale value was analyzed by software.
[0071] like Figure 5 As shown in the figure, on the seventh day after surgery, after the application of hydrogel, the incidence of adhesion in the model rats decreased significantly, the surface of the intestinal wall almost recovered to the level before modeling, and the wound surface of the abdominal wall was smooth and intact, with a little white fibrous tissue hyperplasia. The adhesion score of the hydrogel group was significantly lower than that of the control group, and there was no significant difference with the sham operation group.
[0072] like Figure 6 The pathological sections shown in the figure show that on the seventh day after surgery, the smooth muscle layer, serosal layer of the intestinal wall, mesothelial layer and superficial muscle layer of the abdominal wall of the control group were almost replaced by proliferating fibrous tissue, with a large number of inflammatory cells proliferating, accompanied by neovascularization, and disordered arrangement of the abdominal muscles. The hydrogel group only showed thickening of the abdominal wall mesothelial layer and intestinal wall serosal layer, and the spacing between some intestinal wall smooth muscle layers and submucosal layers became larger. Some broken abdominal muscles were healing, and the surface was re-covered by mesothelial tissue. The sham operation group showed normal abdominal wall and intestinal wall characteristics.
[0073] like Figure 7 As shown, on the seventh day after surgery, the expression level of α-SMA in the intestinal wall and abdominal wall tissue of rats treated with hydrogel was significantly reduced, indicating that the hydrogel has anti-inflammatory and anti-fibrogenic functions.
[0074] This test verified that the hydrogel 1 has good biocompatibility. While promoting cell growth and wound recovery, it resists the adhesion of fibroblasts and blood cells and inhibits the spread of inflammation and excessive growth of fibrous tissue.
[0075] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0076] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a degradation-controllable thermosensitive anti-adhesion hydrogel, It is characterized in that The steps include: Step 1: preparing sodium carboxymethyl cellulose solution; Step 2: adding the sodium carboxymethyl cellulose solution prepared in step 1 to polyether F127 to prepare a degradation-controllable temperature-sensitive anti-adhesion hydrogel; Step 3: The clarified liquid obtained in step 2 is sterilized by high temperature and high pressure sterilization.
2. The method for preparing the degradation-controllable temperature-sensitive anti-adhesion hydrogel according to claim 1, It is characterized in that Step 1: preparing a sodium carboxymethylcellulose solution, comprising the following steps: Sodium carboxymethyl cellulose is added to the solvent and vigorously stirred at 4 to 80° C. for 1 to 8 hours until the sodium carboxymethyl cellulose is completely dissolved, wherein the mass ratio of the sodium carboxymethyl cellulose to deionized water is 1:850 to 1:
24.
3. The method for preparing the degradation-controllable temperature-sensitive anti-adhesion hydrogel according to claim 2, It is characterized in that The solvent is one or more of deionized water, physiological saline, buffer solution, simulated body fluid products, cell culture medium, human body fluid, and animal body fluid.
4. The method for preparing the degradation-controllable temperature-sensitive anti-adhesion hydrogel according to claim 1, It is characterized in that Step 2: preparing a degradation-controllable temperature-sensitive anti-adhesion hydrogel, comprising the following steps: Add the sodium carboxymethyl cellulose solution prepared in step 1 to polyether F127 in a mass ratio of 3:1 to 17:3, and stir vigorously at room temperature for 0.5 to 2 hours until a white paste-like solid is formed. Place the substance in a 4°C refrigerator and let it stand for 8 to 48 hours until it becomes a foamy viscous liquid.
5. The method for preparing the degradation-controllable temperature-sensitive anti-adhesion hydrogel according to claim 1, It is characterized in that Step 3: subjecting the clarified liquid obtained in step 2 to high temperature and high pressure sterilization, comprising the following steps: The clarified liquid obtained in step 2 is placed in an autoclave for high pressure sterilization at 160-180°C for 2-4 hours, then taken out and stored in a refrigerator at 4°C. 6 . A degradation-controllable thermosensitive anti-adhesion hydrogel prepared by the method for preparing the degradation-controllable thermosensitive anti-adhesion hydrogel according to any one of claims 1 to 5 .
7. The degradation-controllable temperature-sensitive anti-adhesion hydrogel according to claim 6, It is characterized in that The polymer network is composed of polyether F127 and carboxymethyl cellulose physically cross-linked.
8. The degradation-controllable temperature-sensitive anti-adhesion hydrogel according to claim 6, It is characterized in that It is in a sol state at 4°C and in a gel state at 37°C.
9. Use of the degradation-controllable thermosensitive anti-adhesion hydrogel according to any one of claims 6 or 8 in the tissue repair of postoperative abdominal adhesion, postoperative pelvic adhesion and other wounds caused by surgical trauma.