High-purity benzyl chloride purification and adsorption material and preparation method thereof

Through the combination of multi-stage pore type ultra-high cross-linked resin matrix and metal-organic framework adsorption materials, the problem of insufficient selectivity and stability of existing high-purity benzyl chloride purification adsorption materials is solved, and efficient benzyl chloride purification is achieved. and long-term stability, meeting the needs of industrial production.

CN118719019APending Publication Date: 2024-10-01CHANGZHOU XINDONG CHEM IND DEV CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410882512.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing high-purity benzyl chloride purification adsorption materials do not have high selectivity, resulting in the adsorption of useful components when removing impurities. The adsorption capacity is limited, and they are easily damaged or lose activity during the regeneration process, resulting in a short service life and unable to meet the needs of industrial production. need.

Method used

Using multi-stage pore type ultra-high cross-linked resin matrix and metal-organic framework adsorption materials, through specific mixing ratios and process treatments, high-purity benzyl chloride purification adsorption materials with high selectivity and stability are prepared, providing good The pore distribution and non-catalytically active functional groups, combined with the micron-sized particle size of the metal-organic framework, improve adsorption performance and stability.

Benefits of technology

It significantly improves the purification efficiency and adsorption capacity of benzyl chloride, extends the service life of the material, ensures the production demand for high-purity benzyl chloride, and provides deep purification and long-term stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004924964580000081
    Figure BDA0004924964580000081
  • Figure BDA0004924964580000091
    Figure BDA0004924964580000091
Patent Text Reader

Abstract

The invention relates to the technical field of high-purity benzyl chloride purification and adsorption materials, in particular to a high-purity benzyl chloride purification and adsorption material and a preparation method thereof. The high-purity benzyl chloride purification and adsorption material comprises a multistage pore diameter type hypercrosslinked resin matrix, and the multistage pore diameter type hypercrosslinked resin matrix is prepared by the following scheme: mixing an oil phase and a water phase, heating, carrying out heat preservation treatment, stirring and mixing, filtering, collecting a filter cake, washing and drying to prepare matrix particles; stirring and mixing the matrix particles, dichloromethane and chloromethyl ethyl ether, performing swelling treatment, adding absolute ethyl alcohol after cross-linking reaction, filtering, washing and drying. The adsorption material has more mesopores and uniform pore distribution, so that a channel is provided for diffusion of adsorbate, the adsorption capacity and the adsorption efficiency of the multistage aperture type hypercrosslinked resin matrix are improved, and the adsorption material is not easy to react in the adsorption and desorption processes, so that the adsorption efficiency of the adsorption material is improved. The long-term stability and the service life are further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-purity benzyl chloride purification adsorption materials, in particular to a high-purity benzyl chloride purification adsorption material and a preparation method thereof. Background Art

[0002] Benzyl chloride is an important organic compound, which is often used as an intermediate in chemical synthesis. In industrial production, the production process of benzyl chloride may be accompanied by the generation of some impurities, which may affect the purity and quality of benzyl chloride. Therefore, purification treatment is required to obtain high-purity benzyl chloride.

[0003] Purification Adsorption is one of the commonly used methods for benzyl chloride purification. In this process, the benzyl chloride solution passes through an adsorbent, usually solid particles or porous materials. These adsorbents are highly selective and can separate impurities from benzyl chloride, thereby improving the purity of benzyl chloride.

[0004] In view of the above-mentioned related technologies, the inventors found that the selectivity of the existing high-purity benzyl chloride purification adsorption materials is not high enough, resulting in the adsorption of some useful components while removing the target impurities, reducing the yield. Secondly, the adsorption capacity of the high-purity benzyl chloride purification adsorption materials is limited. At the same time, the adsorption materials are easily damaged or lose activity during the regeneration process, resulting in poor long-term stability and reusability, which cannot meet production needs. Summary of the invention

[0005] In order to improve the defects of the existing high-purity benzyl chloride purification adsorption material, such as poor adsorption effect and short service life, the present application provides a high-purity benzyl chloride purification adsorption material and a preparation method thereof.

[0006] A high-purity benzyl chloride purification adsorption material and a preparation method thereof, using the following technical scheme:

[0007] A high-purity benzyl chloride purification adsorption material and a preparation method thereof include a multi-level pore size ultra-high cross-linked resin matrix, wherein the multi-level pore size ultra-high cross-linked resin matrix is ​​prepared by the following scheme:

[0008] Take deionized water, gelatin, talcum powder and methylene blue solution, stir and mix, and collect the aqueous phase;

[0009] Then, divinylbenzene, benzoyl peroxide, styrene and paraffin are mixed and stirred, and the oil phase is collected;

[0010] The oil phase and the water phase are mixed and heated, kept warm and stirred, filtered and the filter cake is collected, washed and dried to prepare the matrix particles;

[0011] The matrix particles, dichloromethane and chloromethyl ether are stirred, mixed and swollen, the mixture is collected and a catalyst is added, stirred, mixed and heated for cross-linking reaction, anhydrous ethanol is added to the cross-linking reactant, stirred, mixed and filtered, washed and dried, and the multi-level pore size ultra-high cross-linked resin matrix can be prepared.

[0012] Through the above technical scheme, the present application prepares a multi-level pore size ultra-high cross-linked resin matrix as a high-purity benzyl chloride purification adsorption material. On the one hand, the multi-level pore size ultra-high cross-linked resin matrix has more mesopores and uniform pore distribution, which provides a channel for the diffusion of the adsorbate, improves the adsorption capacity and adsorption efficiency of the multi-level pore size ultra-high cross-linked resin matrix, and also provides a good channel for its effective diffusion; on the other hand, the multi-level pore size ultra-high cross-linked resin matrix prepared by the present application does not contain catalytically active functional groups, and is not easy to react with the adsorbed material during the adsorption and desorption process, further improving its long-term stability and service life.

[0013] Furthermore, the mixing ratio of deionized water, gelatin, talcum powder and methylene blue solution in the aqueous phase is (100-150): (1-1.5): (2.5-3.0): (1-2).

[0014] Furthermore, in the oil phase, the mixing ratio of divinylbenzene, benzoyl peroxide, styrene and paraffin is (100-150):(1-2):(100-150):(100-125).

[0015] Furthermore, the catalyst is a tin tetrachloride catalyst.

[0016] Furthermore, the high-purity benzyl chloride purification adsorption material also includes a metal-organic framework adsorption material filled in a multi-level pore size ultra-high cross-linked resin matrix.

[0017] Furthermore, the metal-organic framework adsorption material includes the following substances in parts by weight:

[0018] 1-2 parts of aluminum nitrate;

[0019] 1.5-3 parts of terephthalic acid;

[0020] 130-150 parts of N,N-dimethylformamide.

[0021] Through the above technical scheme, the present application further adds metal-organic framework adsorption materials into the multi-level pore size ultra-high cross-linked resin matrix for modification. Since the particle size of the metal-organic framework adsorption materials is mostly in the micron level, they can conform to the multi-level pore size ultra-high cross-linked resin matrix to further improve the adsorption performance, and combine ion exchange and specific adsorption to increase the adsorption amount and adsorption rate, thereby deeply adsorbing and purifying benzyl chloride, thereby effectively improving the purification quality of the benzyl chloride material.

[0022] In the second aspect, the present application provides a method for preparing a high-purity benzyl chloride purification adsorption material, using the following technical scheme:

[0023] A method for preparing a high-purity benzyl chloride purification adsorption material comprises the following preparation steps:

[0024] Aluminum nitrate, terephthalic acid and N,N-dimethylformamide are mixed and placed in a reaction device, a multi-level aperture ultra-high cross-linked resin matrix is ​​added and placed in the reaction device, the temperature is raised and kept for reaction, and then the mixture is allowed to stand and cool to room temperature;

[0025] The filter cake is filtered and collected, washed and dried to obtain the metal-organic framework adsorption material.

[0026] Furthermore, the temperature of the heat preservation reaction is 125-140°C.

[0027] Through the above technical scheme, the present application optimizes the preparation method of high-purity benzyl chloride purification adsorption material, and prepares the purification adsorption material with good adsorption performance, high adsorption capacity and long service life through mild reaction conditions.

[0028] In summary, this application has the following beneficial effects:

[0029] First, the present application prepares a multi-level pore size ultra-high cross-linked resin matrix as a high-purity benzyl chloride purification adsorption material. On the one hand, the multi-level pore size ultra-high cross-linked resin matrix has more mesopores and uniform pore distribution, which provides a channel for the diffusion of the adsorbate, improves the adsorption capacity and adsorption efficiency of the multi-level pore size ultra-high cross-linked resin matrix, and also provides a good channel for its effective diffusion; on the other hand, the multi-level pore size ultra-high cross-linked resin matrix prepared in the present application does not contain catalytically active functional groups, and is not easy to react with the adsorbed material during the adsorption and desorption process, further improving its long-term stability and service life.

[0030] Second, the present application further adds metal-organic framework adsorption materials to the multi-level pore size ultra-high cross-linked resin matrix for modification. Since the particle size of the metal-organic framework adsorption materials is mostly in the micron level, they can conform to the multi-level pore size ultra-high cross-linked resin matrix to further improve the adsorption performance. The adsorption amount and adsorption rate are increased by combining ion exchange and specific adsorption, thereby deeply adsorbing and purifying benzyl chloride, thereby effectively improving the purification quality of the benzyl chloride material.

[0031] Third, the present application further modifies the multi-level pore size ultra-high cross-linked resin matrix by further adding a metal-organic framework adsorption material. Since the particle size of the metal-organic framework adsorption material is mostly in the micron level, it can conform to the multi-level pore size ultra-high cross-linked resin matrix to further improve the adsorption performance. The adsorption amount and adsorption rate are increased by combining ion exchange and specific adsorption, thereby deeply adsorbing and purifying benzyl chloride, thereby effectively improving the purification quality of the benzyl chloride material. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments.

[0033] In the examples of the present application, the raw materials and instruments used are as follows, but not limited thereto:

[0034] The present application is further described in detail below with reference to the embodiments.

[0035] Example 1

[0036] Multi-level pore size ultra-high cross-linked resin matrix 1.

[0037] Take 100 g of deionized water, 1 g of gelatin, 2.5 g of talc and 1 g of methylene blue solution, stir and mix, and collect the aqueous phase;

[0038] Then, 125 g of divinylbenzene, 1.5 g of benzoyl peroxide, 118 g of styrene and 125 g of paraffin were stirred and mixed, and the mixture was collected as the oil phase;

[0039] The oil phase and the water phase are mixed and heated to 80°C, kept warm for 3 hours, stirred and mixed, filtered and the filter cake is collected, washed with deionized water, and then dried at 57°C for 24 hours to prepare matrix particles;

[0040] Take 20g of base particles, 225g of dichloromethane, and 7g of chloromethyl ether, stir and mix, and-swell for 3h, collect the mixture and add catalyst tin tetrachloride, stir and mix, heat to 80°C, and keep the cross-linking reaction for 12h, add anhydrous ethanol to the cross-linking reactant, stir and mix, filter, wash and dry, and the multi-level pore size ultra-high cross-linked resin matrix 1 can be prepared as a high-purity benzyl chloride purification adsorption material.

[0041] Example 2

[0042] Multi-level pore size ultra-high cross-linked resin matrix 2.

[0043] Take 125 g of deionized water, 1.3 g of gelatin, 2.7 g of talc and 1.5 g of methylene blue solution and stir to mix, and collect the aqueous phase;

[0044] Then, 125 g of divinylbenzene, 1.45 g of benzoyl peroxide, 118 g of styrene and 125 g of paraffin were stirred and mixed, and the mixture was collected as the oil phase;

[0045] The oil phase and the water phase are mixed and heated to 80°C, kept warm for 3 hours, stirred and mixed, filtered and the filter cake is collected, washed with deionized water, and then dried at 52°C for 24 hours to prepare matrix particles;

[0046] Take 20g of base particles, 225g of dichloromethane, and 7g of chloromethyl ether, stir and mix, and-swell for 3h, collect the mixture and add catalyst tin tetrachloride, stir and mix, heat to 80°C, and keep the cross-linking reaction for 12h, add anhydrous ethanol to the cross-linking reactant, stir and mix, filter, wash and dry, and the multi-level pore size ultra-high cross-linked resin matrix 2 can be prepared as a high-purity benzyl chloride purification adsorption material.

[0047] Example 3

[0048] Multi-level pore size ultra-high cross-linked resin matrix 3.

[0049] Take 150g of deionized water, 1.5g of gelatin, 3.0g of talc and 2g of methylene blue solution and stir to mix, and collect the aqueous phase;

[0050] Then, 150 g of divinylbenzene, 2 g of benzoyl peroxide, 125 g of styrene and 150 g of paraffin were mixed and collected as the oil phase;

[0051] The oil phase and the water phase are mixed and heated to 85°C, kept warm for 4 hours, stirred and mixed, filtered and the filter cake is collected, washed with deionized water, and then dried at 60°C for 24 hours to prepare matrix particles;

[0052] Take 25g of base particles, 250g of dichloromethane, and 8g of chloromethyl ether, stir and mix, and perform swelling treatment for 3h, collect the mixture and add catalyst tin tetrachloride, stir and mix, heat to 85°C, and keep the cross-linking reaction for 12h, add anhydrous ethanol to the cross-linking reactant, stir and mix, filter, wash and dry, and the multi-level pore size ultra-high cross-linked resin matrix 3 can be prepared as a high-purity benzyl chloride purification adsorption material.

[0053] Example 4

[0054] 10 g of aluminum nitrate, 15 g of terephthalic acid and 1300 g of N,N-dimethylformamide were mixed and placed in a reaction device, 20 g of a multi-level aperture ultra-high cross-linked resin matrix 1 was added and placed in the reaction device, the temperature was raised to 125° C. and kept warm for 72 hours, and then allowed to stand and cool to room temperature; the filter cake was filtered and collected, washed and placed at 80° C. for drying for 12 hours, and a high-purity benzyl chloride purification adsorption material was collected.

[0055] Example 5

[0056] 15 g of aluminum nitrate, 22 g of terephthalic acid and 1400 g of N,N-dimethylformamide were mixed and placed in a reaction device, 25 g of a multi-level aperture ultra-high cross-linked resin matrix 1 was added and placed in the reaction device, the temperature was raised to 132° C. and kept warm for 72 hours, and then allowed to stand and cool to room temperature; the filter cake was filtered and collected, washed and placed at 80° C. for drying for 12 hours, and a high-purity benzyl chloride purification adsorption material was collected.

[0057] Example 6

[0058] Take 20g of aluminum nitrate, 30g of terephthalic acid and 1500g of N,N-dimethylformamide, stir and mix them and place them in a reaction device, add 30g of multi-level pore size ultra-high cross-linked resin matrix 1 and place it in the reaction device, heat it to 140°C and keep it warm for 72 hours, then stand and cool to room temperature; filter and collect the filter cake, wash it and place it at 80°C for drying for 12 hours to collect high-purity benzyl chloride purification adsorption material.

[0059] Example 7

[0060] 15 g of aluminum nitrate, 22 g of terephthalic acid and 1400 g of N,N-dimethylformamide were mixed and placed in a reaction device, 25 g of a multi-level aperture ultra-high cross-linked resin matrix 2 was added and placed in the reaction device, the temperature was raised to 132° C. and the reaction was kept warm for 72 hours, and then the mixture was allowed to stand and cool to room temperature; the filter cake was filtered and collected, washed and dried at 80° C. for 12 hours, and a high-purity benzyl chloride purification adsorption material was collected.

[0061] Example 8

[0062] 15 g of aluminum nitrate, 22 g of terephthalic acid and 1400 g of N,N-dimethylformamide were mixed and placed in a reaction device, 25 g of a multi-level aperture ultra-high cross-linked resin matrix 3 was added and placed in the reaction device, the temperature was raised to 132° C. and kept warm for 72 hours, and then allowed to stand and cool to room temperature; the filter cake was filtered and collected, washed and placed at 80° C. for drying for 12 hours, and a high-purity benzyl chloride purification adsorption material was collected.

[0063] Performance Testing

[0064] The performance of the high-purity benzyl chloride purification adsorption material prepared in Examples 1-8 was tested:

[0065] Take 10g of high-purity benzyl chloride purification adsorption material and put it into an adsorption device with a size of 20mL. The benzyl chloride raw material (toluene content 250ppm, o-chlorotoluene content 250ppm, p-chlorotoluene content 190ppm, benzaldehyde content 650ppm, and other impurities 3780ppm) enters the U-shaped tube at a speed of 5mL / h using a syringe pump. After 180 minutes, the contents of o-chlorotoluene, p-chlorotoluene, toluene, benzaldehyde and other impurities are collected on the other side of the raw material injection point, and the content of stored benzyl chloride is measured. The details are shown in Table 1 below:

[0066] The details are shown in Table 1 below:

[0067] Table 1 Performance test table

[0068]

[0069]

[0070] From the results of the above-mentioned Examples 1-8 and Table 1, it can be found that: the present application prepares a multi-level pore size ultra-high cross-linked resin matrix as a high-purity benzyl chloride purification adsorption material. On the one hand, the multi-level pore size ultra-high cross-linked resin matrix has more mesopores and uniform pore distribution, which provides a channel for the diffusion of the adsorbate, improves the adsorption capacity and adsorption efficiency of the multi-level pore size ultra-high cross-linked resin matrix, and also provides a good channel for its effective diffusion; on the other hand, the multi-level pore size ultra-high cross-linked resin matrix prepared in the present application does not contain catalytically active functional groups, and is not easy to react with the adsorbed material during the adsorption and desorption process, further improving its long-term stability and service life.

[0071] By comparing Examples 1-3 with Examples 4-8, it is further illustrated that the present application further adds a metal-organic framework adsorption material to the multi-level pore size ultra-high cross-linked resin matrix for modification. Since the particle size of the metal-organic framework adsorption material is mostly in the micron level, it can conform to the multi-level pore size ultra-high cross-linked resin matrix to further improve the adsorption performance. The adsorption amount and adsorption rate are increased by combining ion exchange and specific adsorption, thereby deeply adsorbing and purifying benzyl chloride, thereby effectively improving the purification quality of the benzyl chloride material.

[0072] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0073] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.

[0074] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0075] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.

Claims

1. A high-purity benzyl chloride purification adsorption material, It is characterized in that It comprises a multi-level pore size ultra-high cross-linked resin matrix, and the multi-level pore size ultra-high cross-linked resin matrix is ​​made by the following scheme: Take deionized water, gelatin, talcum powder and methylene blue solution, stir and mix, and collect the aqueous phase; Then, divinylbenzene, benzoyl peroxide, styrene and paraffin are mixed and stirred, and the oil phase is collected; The oil phase and the water phase are mixed and heated, kept warm and stirred, filtered and the filter cake is collected, washed and dried to prepare the matrix particles; The matrix particles, dichloromethane and chloromethyl ether are stirred, mixed and swollen, the mixture is collected and a catalyst is added, stirred, mixed and heated for cross-linking reaction, anhydrous ethanol is added to the cross-linking reactant, stirred, mixed and filtered, washed and dried, and the multi-level pore size ultra-high cross-linked resin matrix can be prepared.

2. A high-purity benzyl chloride purification adsorption material according to claim 1, It is characterized in that The mixing ratio of deionized water, gelatin, talcum powder and methylene blue solution in the aqueous phase is (100-150): (1-1.5): (2.5-3.0): (1-2).

3. A high-purity benzyl chloride purification adsorption material according to claim 1, It is characterized in that In the oil phase, the mixing ratio of divinylbenzene, benzoyl peroxide, styrene and paraffin is (100-150):(1-2):(100-150):(100-125).

4. A high-purity benzyl chloride purification adsorption material according to claim 1, It is characterized in that The catalyst is a tin tetrachloride catalyst.

5. A high-purity benzyl chloride purification adsorption material according to claim 1, It is characterized in that The high-purity benzyl chloride purification adsorption material also includes a metal-organic framework adsorption material filled in a multi-level pore size ultra-high cross-linked resin matrix.

6. A high-purity benzyl chloride purification adsorption material according to claim 5, It is characterized in that The metal-organic framework adsorption material comprises the following substances in parts by weight: 1-2 parts of aluminum nitrate; 1.5-3 parts of terephthalic acid; 130-150 parts of N,N-dimethylformamide.

7. A method for preparing a high-purity benzyl chloride purification adsorption material according to any one of claims 1 to 6, It is characterized in that The method comprises the following preparation steps: Aluminum nitrate, terephthalic acid and N,N-dimethylformamide are mixed and placed in a reaction device, a multi-level aperture ultra-high cross-linked resin matrix is ​​added and placed in the reaction device, the temperature is raised and kept for reaction, and then the mixture is allowed to stand and cool to room temperature; The filter cake is filtered and collected, washed and dried to obtain the metal-organic framework adsorption material.

8. A method for preparing a high-purity benzyl chloride purification adsorption material according to claim 7, It is characterized in that The temperature of the heat preservation reaction is 125-140°C.

Citation Information

Patent Citations

  • Bifunctional hierarchical porous adsorbent resin and preparation method thereof

    CN109337004A

  • Resin-based hybrid material based on zirconium-based metal organic framework modification and application thereof

    CN111530427A

  • Preparation method of adsorption resin for purifying volatile organic compounds

    CN115487789A

  • Method for treating volatile organic compounds by adopting hypercrosslinked adsorption resin

    CN115845555A