CuO-SrO / Mn x Zr 1-x O 2 Composite oxygen carrier and its preparation method and application

Through the use of CuO-SrO/MnxZr1-xO2 composite oxygen carrier catalyst, the lattice oxygen oxidation and decomposition problem of the risk and low yield of oxygen inflow in the ammonia decomposition process is solved, and high-efficiency hydrogen production and Recycling of catalysts.

CN118719038BActive Publication Date: 2024-11-05WEIFANG MEDICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411215391.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-05
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

In the existing ammonia decomposition process, the inflow of oxygen is high, strict operating requirements and strong oxidation, resulting in a reduced hydrogen yield.

Method used

The CuO-SrO/MnxZr1-xO2 composite oxygen carrier is used as a catalyst to decompose the lattice oxygen oxidation, which avoids the direct inflow of oxygen, improves the hydrogen yield, and the oxygen carrier can be recycled multiple times.

Benefits of technology

It improves the conversion rate and hydrogen yield of ammonia gas decomposition, reduces the risk of equipment explosion, and maintains the stability and durability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719038B_ABST
    Figure CN118719038B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of preparation and application of oxygen carriers, and specifically relates to CuO-SrO / Mn x Zr 1‑x O2 composite oxygen carrier and its preparation method and application. The preparation method of the composite oxygen carrier is as follows: Mn(NO3)2·6H2O and ZrO(NO3)2·2H2O are dissolved in water, mixed, pH is adjusted, and calcined to obtain Mn x Zr 1‑x O2 powder is dissolved in water, Cu(NO3)2•3H2O and Sr(NO3)2•4H2O are added, mixed evenly, a precipitant is added, stirred, the solid obtained is ground and calcined to obtain a composite oxygen carrier. The present invention provides CuO-SrO / Mn x Zr 1‑x The invention discloses a method for preparing an O2 composite oxygen carrier. The prepared composite oxygen carrier has a large specific surface area and many oxygen vacancies and is used for decomposing ammonia. The composite oxygen carrier can be recycled for multiple times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of preparation and application of oxygen carriers, and specifically relates to CuO-SrO / Mn x Zr 1-x O2 composite oxygen carrier and its preparation method and application. Background Art

[0002] Hydrogen is a clean energy source, but its transportation and storage remain a major challenge. To address this issue, researchers have been exploring catalytic NH3 decomposition as an alternative method for producing hydrogen. In the past decade, ammonia decomposition has received great attention as a promising method for producing CO-free hydrogen using green energy. Ammonia decomposition to produce hydrogen is currently widely used due to its relatively mature technology. The process has the advantages of simplicity, high energy density, easy storage, and safety. In the preparation of hydrogen from ammonia, ammonia needs to be catalytically decomposed by thermal catalysis to obtain hydrogen. The thermal catalysis requires the use of a thermal catalyst, and the catalyst generally selected is a transition metal nitride. Strontium-based catalysts have a unique ability to store oxygen and disperse surface active components, which makes many aerobic reactions have high low-temperature activity. It has been reported in the literature that the reduction of supported metal catalysts (such as Rh / CeO 2-x and Rh / Ce 0.5 Zr 0.5 O 2-x ) The heat generated by oxidation can be used to trigger the oxidative reforming of hydrocarbons. Similarly, catalysts used in the process of hydrogen production by ammonia oxidation decomposition, such as Ru / Al2O3, Ru / Ce 0.5 Zr 0.5 O 2-x There are also reports, but its application is limited due to its high cost, low reserves of precious metals, and serious environmental pollution.

[0003] At present, the decomposition process of NH3 is mainly ensured by introducing oxygen into the process, but the introduction of oxygen has the following main disadvantages: first, the introduction of oxygen has a high risk factor, which increases the risk of the process. If the oxygen is further controlled to prevent explosion, the operation requirements of the process are strict and the stability is poor. Second, due to the strong oxidizing property of O2, the product H2 is easily oxidized to generate H2O, reducing the yield of H2.

[0004] Japanese patent JP2014159031A discloses a catalyst for producing hydrogen, and a method for producing hydrogen using the catalyst, wherein the catalyst for producing hydrogen for decomposing ammonia containing ammonia and oxygen to produce hydrogen contains at least one selected from cobalt, nickel, iron and molybdenum as a catalyst component. Alkali metals, alkaline earth metals or rare earth elements can be added to the catalyst. At least one metal oxide selected from aluminum oxide, silicon dioxide, zirconium oxide, titanium dioxide, cerium dioxide, lanthanum oxide, magnesium oxide, calcium oxide, barium oxide and strontium oxide can be introduced into the catalyst. This reaction requires the addition of oxygen to increase the decomposition rate of ammonia, but oxygen has a strong oxidizing property, and the H2 after the decomposition of ammonia reacts with O2 to generate H2O, which will reduce the yield of H2. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a CuO-SrO / Mn x Zr 1-x The invention discloses a method for preparing an O2 composite oxygen carrier. The prepared composite oxygen carrier has a large specific surface area and many oxygen vacancies. The composite oxygen carrier is applied to decompose ammonia to produce hydrogen. The composite oxygen carrier can be recycled for multiple times, and has a high ammonia conversion rate and a high hydrogen yield.

[0006] The CuO-SrO / Mn x Zr 1-x The preparation method of O2 composite oxygen carrier comprises the following steps:

[0007] (1) Dissolve Mn(NO3)2·6H2O and ZrO(NO3)2·2H2O in water respectively, then mix the two solutions, adjust the pH of the solution to 7-9, stir at room temperature, filter, wash, dry, and calcine to obtain Mn x Zr 1-x O2 powder;

[0008] (2) Mn x Zr 1-x O2 powder is ground to a particle size of 100-500 μm;

[0009] (3) The Mn ground in step (2) x Zr 1-x O2 is dissolved in water, Cu(NO3)2•3H2O and Sr(NO3)2•4H2O are added, mixed evenly, a precipitant is added, stirred at 60-100℃ for 6-12h, allowed to stand for precipitation, filtered, washed, dried, the obtained solid is ground to 100-500μm, calcined, and CuO-SrO / Mn is obtained. x Zr 1-x O2 composite oxygen carrier;

[0010] Mn xZr 1-x The mass ratio of O2, Cu(NO3)2•3H2O, and Sr(NO3)2•4H2O is (1:5:5)-(8:1:3).

[0011] The x in step (1) is 0.2, 0.4, 0.6, and 0.8.

[0012] In step (1), pH is adjusted by using one of ammonia water, sodium hydroxide and potassium hydroxide, with a mass concentration of 25%-30%.

[0013] The drying temperature of step (1) is 60-100°C and the drying time is 8-16h.

[0014] The calcination temperature of step (1) is 650-850°C, and the calcination time is 4-8h.

[0015] The precipitant in step (3) is thiourea or urea, 20-200 mg of which is added to every 100-500 mL of water.

[0016] The drying temperature of step (3) is 60-100°C and the drying time is 8-16h.

[0017] The calcination atmosphere in step (3) is argon or helium. The calcination is carried out in a tubular furnace at a temperature of 450-650° C. for a time of 3-6 hours.

[0018] A CuO-SrO / Mn x Zr 1-x The O2 composite oxygen carrier is composed of the CuO-SrO / Mn x Zr 1-x The invention is prepared by the preparation method of O2 composite oxygen carrier.

[0019] A CuO-SrO / Mn x Zr 1-x The application of O2 composite oxygen carrier includes the following steps:

[0020] a. Put CuO-SrO / Mn x Zr 1-x Add O2 composite oxygen carrier into the fixed bed reactor and pre-treat it with nitrogen at a flow rate of 100-250mL / min for 30-50min (to exhaust the air and water vapor in the reactor). Set the temperature of the preheater and the fixed bed reactor. The preheater is set at 100-400℃, and the fixed bed reactor is set at 200-500℃. Heat up and set the reaction pressure to 0.3-1MPa (although pressurization is not conducive to the decomposition of ammonia, it is for the purpose of improving mass transfer and reaction rate).

[0021] b. Set the ammonia inlet flow rate to 50-60 mL / min to obtain hydrogen as a gas phase product.

[0022] c. After the reaction is completed, nitrogen is introduced to exhaust the H2 in the reactor. At the same time, the oxygen carrier that has lost lattice oxygen after the reaction continues to introduce oxygen in the fixed bed. The fixed bed reactor is set at a temperature of 300-550℃ to make CuO-SrO / Mn x Zr 1-x O2 composite oxygen carrier restores lattice oxygen.

[0023] Specifically, the CuO-SrO / Mn x Zr 1-x The preparation method of O2 composite oxygen carrier comprises the following steps:

[0024] (1) Dissolve Mn(NO3)2·6H2O and ZrO(NO3)2·2H2O solid particles in 200 mL of deionized water and stir for 30 min, then mix the two solutions and stir for another 30 min, adjust the pH of the solution to 7-9 with 25%-30% of a regulator, stir the mixed solution at room temperature for 12 h, filter, wash, and then dry at 60-100°C for 8-16 h, and calcine at 650-850°C in a tube furnace under argon or helium for 4-8 h to obtain Mn x Zr 1-x O2 powder, x is 0.2, 0.4, 0.6, 0.8; (the doping of Zr in the manganese oxide framework increases the specific surface area of ​​the oxygen carrier and increases the oxygen vacancies, thereby promoting the oxidation and decomposition of NH3).

[0025] (2) Mn x Zr 1-x O2 powder was ground to a particle size of 100-500 μm.

[0026] (3) The Mn ground in step (2) x Zr 1-x O2 was dissolved in 100-500 mL of deionized water and stirred for 30 min. Cu(NO3)2•3H2O and Sr(NO3)2•4H2O solid particles were added and stirred for 2 h. After uniform mixing, 20-200 mg of precipitant thiourea was added and stirred at 60-100 °C for 6-12 h. The mixture was precipitated at room temperature for 12 h. The mixture was filtered, washed, and dried at 60-100 °C for 8-16 h. The obtained solid was ground to 100-500 μm and calcined at 450-650 °C in a tube furnace in argon or helium for 3-6 h to obtain CuO-SrO / Mn x Zr 1-x O2 composite oxygen carrier; Mn x Zr 1-xThe mass ratio of O2, Cu(NO3)2•3H2O, and Sr(NO3)2•4H2O is (1:5:5)-(8:1:3). The present invention uses lattice oxygen in the oxygen carrier to catalytically oxidize ammonia into H2. At the same time, the lattice oxygen in the oxygen carrier has a weak oxidizing property and is not easy to oxidize the H2 produced after the decomposition of ammonia, thereby greatly improving the yield of H2 and avoiding the risk of equipment explosion caused by the introduction of O2.

[0027] The present invention introduces zirconium oxide (ZrO2) to form a solid solution carrier Mn x Zr 1-x O2 improves the thermal stability of the material. Mn in the ZrO2 lattice 4+ Ion substitution Zr 4+ Ions are its stabilization mechanism. Zr 4+ With Mn 4+ Smaller ionic radius, resulting in the presence of oxygen vacancies in the lattice to maintain charge balance. These oxygen vacancies improve the ionic conductivity of the material and prevent phase changes that may occur in pure ZrO2 at high temperatures, making it more stable. Zirconia is highly refractory and has excellent thermal stability, while manganese oxide has oxygen storage capacity and redox properties. By combining these properties, manganese-zirconium mixed oxides exhibit better heat resistance and enhanced redox behavior. The improved thermal stability of manganese oxide-zirconium oxide mixed oxides allows them to maintain structural integrity even at high temperatures, mitigating sintering effects. This property is critical for catalytic applications, where stability and durability are essential. In addition, the redox properties of these mixed oxides enhance catalytic activity, especially at lower temperatures. The oxygen storage capacity of zirconium oxide and the stability of zirconium oxide promote efficient redox reactions and facilitate the catalytic process. Mn x Zr 1-x O2 solid solution is a key component of the catalyst. The introduction of smaller Zr into the MnO2 lattice 4+ The cations generate rich surfaces and abundant oxygen vacancies, which play an important role in improving the catalytic performance.

[0028] In the current NH3 decomposition process, in order to promote the decomposition of ammonia, O2 is usually introduced into the reactor. Since O2 has a strong oxidizing property, it is easy to oxidize the product H2 to generate H2O, thereby reducing the yield of H2. However, the present invention uses lattice oxygen to oxidize ammonia. The oxidizing property of lattice oxygen is much lower than that of O2, and it is not easy to oxidize H2, thereby greatly improving the yield of the product H2.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) CuO-SrO / Mn x Zr 1-xThe preparation method of O2 composite oxygen carrier has simple process and the prepared composite oxygen carrier can be recycled.

[0031] (2) CuO-SrO / Mn prepared by the method of the present invention x Zr 1-x O2 composite oxygen carrier has a large specific surface area and many oxygen vacancies, which increases the catalytic effect.

[0032] (3) CuO-SrO / Mn prepared by the present invention x Zr 1-x O2 composite oxygen carrier is used in ammonia decomposition, which makes the conversion rate of NH3 high and the yield of H2 high. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The CuO-SrO / Mn of Example 1 x Zr 1-x Surface TEM image of O2 composite oxygen carrier. DETAILED DESCRIPTION

[0034] The present invention will be further described below in conjunction with specific embodiments.

[0035] The raw materials and auxiliary agents used in the following examples and comparative examples are all commercially available. The pH adjustment described below is not recorded in the examples, as long as it is within the range after adding the adjusting agent. The grinding to particle size described above is not further recorded as long as the particle size in the examples is within the specified range.

[0036] Example 1

[0037] The CuO-SrO / Mn 0.2 Zr 0.8 The preparation method of O2 composite oxygen carrier comprises the following steps:

[0038] (1) 57.4 mg of Mn(NO3)2·6H2O and 213.6 mg of ZrO(NO3)2·2H2O solid particles were dissolved in 500 mL of deionized water and stirred for 30 min, then the two solutions were mixed and stirred for another 30 min, the pH was adjusted to 7-9 with 25% ammonia solution, the mixed solution was stirred at room temperature for 12 h, filtered, washed, and then dried at 80 °C for 10 h, and calcined at 800 °C in an argon atmosphere in a tube furnace for 6 h to obtain Mn 0.2 Zr 0.8 O2 powder.

[0039] (2) Mn 0.2 Zr 0.8 O2 powder was ground to a particle size of 100-500 μm.

[0040] (3) The 115.8 mg Mn 0.2 Zr 0.8 O2 was dissolved in 300 mL of deionized water and stirred for 30 min. 579 mg of Cu(NO3)2•3H2O and 579 mg of Sr(NO3)2•4H2O solid particles were added and stirred for 2 h. After mixing evenly, 20 mg of precipitant thiourea was added and stirred at 80 °C for 8 h. The mixture was precipitated at room temperature for 12 h. The mixture was filtered, washed, and dried at 90 °C for 10 h. The obtained solid was ground to 100-500 μm and calcined at 500 °C in a tube furnace for 4 h in an argon atmosphere to obtain CuO-SrO / Mn 0.2 Zr 0.8 O2 composite oxygen carrier. Its surface TEM image is as follows Figure 1 shown.

[0041] Example 2

[0042] The CuO-SrO / Mn 0.4 Zr 0.6 The preparation method of O2 composite oxygen carrier comprises the following steps:

[0043] (1) 115 mg of Mn(NO3)2·6H2O and 160.2 mg of ZrO(NO3)2·2H2O solid particles were dissolved in 500 mL of deionized water and stirred for 30 min, then the two solutions were mixed and stirred for another 30 min, the pH was adjusted to 7-9 with 30% sodium hydroxide solution, the mixed solution was stirred at room temperature for 12 h, filtered, washed, and then dried at 100 °C for 8 h, and calcined at 850 °C in an argon atmosphere in a tube furnace for 4 h to obtain Mn 0.4 Zr 0.6 O2 powder.

[0044] (2) Mn 0.4 Zr 0.6 O2 powder was ground to a particle size of 100-500 μm.

[0045] (3) The 108.6 mg Mn 0.4 Zr 0.6 O2 was dissolved in 300 mL of deionized water and stirred for 30 min. 162.9 mg Cu(NO3)2•3H2O and 271.5 mg Sr(NO3)2•4H2O solid particles were added and stirred for 2 h. After mixing evenly, 20 mg of precipitant thiourea was added and stirred at 100 °C for 6 h. The mixture was precipitated at room temperature for 12 h. The mixture was filtered, washed, and dried at 100 °C for 8 h. The obtained solid was ground to 100-500 μm and calcined at 450 °C in a tube furnace in an argon atmosphere for 6 h to obtain CuO-SrO / Mn 0.4 Zr 0.6O2 composite oxygen carrier.

[0046] Example 3

[0047] The CuO-SrO / Mn 0.6 Zr 0.4 The preparation method of O2 composite oxygen carrier comprises the following steps:

[0048] (1) 172.2 mg of Mn(NO3)2·6H2O and 106.8 mg of ZrO(NO3)2·2H2O solid particles were dissolved in 500 mL of deionized water and stirred for 30 min, then the two solutions were mixed and stirred for another 30 min, the pH was adjusted to 7-9 with 30% potassium hydroxide solution, the mixed solution was stirred at room temperature for 12 h, filtered, washed, and then dried at 60 °C for 16 h, and calcined at 650 °C in a tube furnace in a helium atmosphere for 8 h to obtain Mn 0.6 Zr 0.4 O2 powder.

[0049] (2) Mn 0.6 Zr 0.4 O2 was ground to a particle size of 100-500 μm.

[0050] (3) The 101.4 mg Mn 0.6 Zr 0.4 O2 was dissolved in 300 mL of deionized water and stirred for 30 min. 67.6 mg Cu(NO3)2•3H2O and 67.6 mg Sr(NO3)2•4H2O solid particles were added and stirred for 2 h. After mixing evenly, 20 mg of urea as a precipitant was added and stirred at 60 °C for 12 h. The mixture was precipitated at room temperature for 12 h. The mixture was filtered, washed, and dried at 100 °C for 8 h. The obtained solid was ground to 100-500 μm and calcined at 650 °C in a tubular furnace for 3 h in a helium atmosphere to obtain CuO-SrO / Mn 0.6 Zr 0.4 O2 composite oxygen carrier.

[0051] Example 4

[0052] The CuO-SrO / Mn 0.8 Zr 0.2 The preparation method of O2 composite oxygen carrier comprises the following steps:

[0053] (1) 223 mg of Mn(NO3)2·6H2O and 53.4 mg of ZrO(NO3)2·2H2O solid particles were dissolved in 500 mL of deionized water and stirred for 30 min, then the two solutions were mixed and stirred for another 30 min, the pH was adjusted to 7-9 with 30% ammonia solution, the mixed solution was stirred at room temperature for 12 h, filtered, washed, and then dried at 90 °C for 9 h, and calcined at 750 °C in a tube furnace under a helium atmosphere for 7 h to obtain Mn 0.8 Zr 0.2 O2 powder.

[0054] (2) Mn 0.8 Zr 0.2 O2 powder was ground to a particle size of 100-500 μm.

[0055] (3) The 94.2 mg Mn 0.8 Zr 0.2 O2 was dissolved in 300 mL of deionized water and stirred for 30 min. 11.7 mg Cu(NO3)2•3H2O and 35.3 mg Sr(NO3)2•4H2O solid particles were added and stirred for 2 h. After mixing evenly, 50 mg of precipitant thiourea was added and stirred at 70 °C for 10 h. The mixture was precipitated at room temperature for 12 h. The mixture was filtered, washed, and dried at 60 °C for 16 h. The obtained solid was ground to 100-500 μm and calcined at 550 °C in a tube furnace for 4 h in a helium atmosphere to obtain CuO-SrO / Mn 0.8 Zr 0.2 O2 composite oxygen carrier.

[0056] Example 5

[0057] The CuO-SrO / Mn prepared in Example 1 0.2 Zr 0.8 The O2 composite oxygen carrier is used to decompose ammonia to prepare hydrogen, including the following steps:

[0058] a. Add 50mgCuO-SrO / Mn 0.2 Zr 0.8 The O2 composite oxygen carrier was added to the fixed bed reactor and pretreated with nitrogen at a flow rate of 100 mL / min for 50 minutes. The temperatures of the preheater and the fixed bed reactor were set. The preheater was set to 200°C, and the reaction temperature of the fixed bed reactor was set to 300°C. The temperature was increased and the reaction pressure was set to 0.5 MPa.

[0059] b. Set the ammonia inlet flow rate to 60 mL / min to obtain hydrogen as a gas phase product.

[0060] c. After the reaction is completed, nitrogen is introduced to exhaust the H2 in the reactor. At the same time, the oxygen carrier that has lost lattice oxygen after the reaction continues to introduce oxygen in the fixed bed. The fixed bed reactor is set at 500°C to make CuO-SrO / Mn 0.2 Zr 0.8 O2 composite oxygen carrier restores lattice oxygen.

[0061] Example 6

[0062] The CuO-SrO / Mn prepared in Example 2 0.4 Zr 0.6 The O2 composite oxygen carrier is used to decompose ammonia to prepare hydrogen, including the following steps:

[0063] a. Add 50mgCuO-SrO / Mn 0.4 Zr 0.6 The O2 composite oxygen carrier was added to the fixed bed reactor and pretreated with nitrogen at a flow rate of 200 mL / min for 30 minutes. The temperatures of the preheater and the fixed bed reactor were set. The preheater was set to 400°C, and the reaction temperature of the fixed bed reactor was set to 500°C. The temperature was increased and the reaction pressure was set to 1 MPa.

[0064] b. Set the ammonia inlet flow rate to 60 mL / min to obtain hydrogen as a gas phase product.

[0065] c. After the reaction is completed, nitrogen is introduced to exhaust the H2 in the reactor. At the same time, the oxygen carrier that has lost lattice oxygen after the reaction continues to introduce oxygen in the fixed bed. The fixed bed reactor is set at 300°C to make CuO-SrO / Mn 0.4 Zr 0.6 O2 composite oxygen carrier restores lattice oxygen.

[0066] Example 7

[0067] The CuO-SrO / Mn prepared in Example 3 0.6 Zr 0.4 The O2 composite oxygen carrier is used to decompose ammonia to prepare hydrogen, including the following steps:

[0068] a. Add 50mgCuO-SrO / Mn 0.6 Zr 0.4 The O2 composite oxygen carrier was added to the fixed bed reactor and pretreated with nitrogen at a flow rate of 100 mL / min for 30 minutes. The temperatures of the preheater and the fixed bed reactor were set. The preheater was set to 100°C, and the reaction temperature of the fixed bed reactor was set to 200°C. The temperature was increased and the reaction pressure was set to 0.3 MPa.

[0069] b. Set the ammonia inlet flow rate to 50 mL / min to obtain hydrogen as a gas phase product.

[0070] c. After the reaction is completed, nitrogen is introduced to exhaust the H2 in the reactor. At the same time, the oxygen carrier that has lost lattice oxygen after the reaction continues to introduce oxygen in the fixed bed. The fixed bed reactor is set at 400°C to make CuO-SrO / Mn 0.6 Zr 0.4 O2 composite oxygen carrier restores lattice oxygen.

[0071] Example 8

[0072] The CuO-SrO / Mn prepared in Example 4 0.8 Zr 0.2 The O2 composite oxygen carrier is used to decompose ammonia to prepare hydrogen, including the following steps:

[0073] a. Add 50mgCuO-SrO / Mn 0.8 Zr 0.2 The O2 composite oxygen carrier was added to the fixed bed reactor and pretreated with nitrogen at a flow rate of 250 mL / min for 45 minutes. The temperatures of the preheater and the fixed bed reactor were set. The preheater was set to 300°C, and the reaction temperature of the fixed bed reactor was set to 400°C. The temperature was increased and the reaction pressure was set to 0.7 MPa.

[0074] b. Set the ammonia inlet flow rate to 60 mL / min to obtain hydrogen as a gas phase product.

[0075] c. After the reaction is completed, nitrogen is introduced to exhaust the H2 in the reactor. At the same time, the oxygen carrier that has lost lattice oxygen after the reaction continues to introduce oxygen in the fixed bed. The fixed bed reactor is set at 550°C to make CuO-SrO / Mn 0.8 Zr 0.2 The O2 composite oxygen carrier recovers lattice oxygen. The cycle experiment was repeated 10 times. The experimental results are shown in Table 3.

[0076] Comparative Example 1

[0077] A Mn 0.2 Zr 0.8 The preparation method of O2 oxygen carrier comprises the following steps:

[0078] 57.4 mg of Mn(NO3)2·6H2O and 213.6 mg of ZrO(NO3)2·2H2O solid particles were dissolved in 500 mL of deionized water and stirred for 30 min, and then the two solutions were mixed and stirred for another 30 min. The pH was adjusted to 7-9 with 25% ammonia solution, and the mixed solution was stirred at room temperature for 12 h, filtered, washed, and then dried at 80 °C for 10 h to obtain Mn 0.2 Zr 0.8 O2 powder.

[0079] Comparative Example 2

[0080] A CuO / Mn 0.2 Zr 0.8 The preparation method of O2 oxygen carrier comprises the following steps:

[0081] (1) 57.4 mg of Mn(NO3)2·6H2O and 213.6 mg of ZrO(NO3)2·2H2O solid particles were dissolved in 500 mL of deionized water and stirred for 30 min, then the two solutions were mixed and stirred for another 30 min, the pH was adjusted to 7-9 with 25% ammonia solution, the mixed solution was stirred at room temperature for 12 h, filtered, washed, and then dried at 80 °C for 10 h, and calcined at 800 °C in an argon atmosphere in a tube furnace for 6 h to obtain Mn 0.2 Zr 0.8 O2 powder.

[0082] (2) Mn 0.2 Zr 0.8 O2 powder was ground to a particle size of 100-500 μm.

[0083] (3) The 115.8 mg Mn 0.2 Zr 0.8 O2 was dissolved in 300 mL of deionized water and stirred for 30 min, 579 mg of Cu(NO3)2•3H2O solid particles were added and stirred for 2 h. After mixing evenly, 100 mg of precipitant thiourea was added and stirred at 80 °C for 8 h. The mixture was precipitated at room temperature for 12 h, filtered, washed, and dried at 90 °C for 10 h. The obtained solid was ground to 100-500 μm and calcined at 500 °C in a tube furnace in an argon atmosphere for 4 h to obtain CuO / Mn 0.2 Zr 0.8 O2 oxygen carrier.

[0084] Comparative Example 3

[0085] A SrO / Mn 0.2 Zr 0.8 The preparation method of O2 oxygen carrier comprises the following steps:

[0086] (1) 57.4 mg of Mn(NO3)2·6H2O and 213.6 mg of ZrO(NO3)2·2H2O solid particles were dissolved in 500 mL of deionized water and stirred for 30 min, then the two solutions were mixed and stirred for another 30 min, the pH was adjusted to 7-9 with 25% ammonia solution, the mixed solution was stirred at room temperature for 12 h, filtered, washed, and then dried at 80 °C for 10 h, and calcined at 800 °C in an argon atmosphere in a tube furnace for 6 h to obtain Mn 0.2 Zr 0.8 O2 powder.

[0087] (2) Mn0.2 Zr 0.8 O2 powder was ground to a particle size of 100-500 μm.

[0088] (3) The 115.8 mg Mn 0.2 Zr 0.8 O2 was dissolved in 300 mL of deionized water and stirred for 30 min. 579 mg of Sr(NO3)2•4H2O solid particles were added and stirred for 2 h. After mixing evenly, 100 mg of precipitant thiourea was added and stirred at 80 °C for 8 h. The mixture was precipitated at room temperature for 12 h. The mixture was filtered, washed, and dried at 90 °C for 10 h. The obtained solid was ground to 100-500 μm and calcined at 500 °C in a tube furnace for 4 h in an argon atmosphere to obtain SrO / Mn 0.2 Zr 0.8 O2 oxygen carrier.

[0089] Comparative Example 4

[0090] The preparation method of the CuO-SrO / MnO2 composite oxygen carrier comprises the following steps:

[0091] (1) Dissolve 287 mg of Mn(NO3)2·6H2O solid particles in 500 mL of deionized water and stir for 30 min. Then mix the two solutions and stir for another 30 min. Adjust the pH to 7-9 with 25% ammonia solution. Stir the mixed solution at room temperature for 12 h, filter, wash, and then dry at 80 °C for 10 h. Calcine at 800 °C in a tube furnace under argon atmosphere for 6 h to obtain MnO2 powder.

[0092] (2) Grind the MnO2 powder to a particle size of 100-500 μm.

[0093] (3) Dissolve 87 mg of MnO2 ground in step (2) in 300 mL of deionized water and stir for 30 min, add 435 mg of Cu(NO3)2•3H2O and 435 mg of Sr(NO3)2•4H2O solid particles and stir for 2 h. Mix well, add 20 mg of precipitant thiourea, stir at 80 °C for 8 h, precipitate at room temperature for 12 h, filter, wash, and dry at 90 °C for 10 h. Grind the obtained solid to 100-500 μm, and calcine at 500 °C in an argon atmosphere in a tube furnace for 4 h to obtain CuO-SrO / Mn 0.2 Zr 0.8 O2 composite oxygen carrier.

[0094] Comparative Example 5

[0095] The preparation method of the CuO-SrO / ZrO2 composite oxygen carrier comprises the following steps:

[0096] (1) Dissolve 267 mg ZrO(NO3)2·2H2O solid particles in 500 mL deionized water and stir for 30 min. Then mix the two solutions and stir for another 30 min. Adjust the pH to 7-9 with 25% ammonia solution. Stir the mixed solution at room temperature for 12 h, filter, wash, and then dry at 80 °C for 10 h. Calcine at 800 °C in a tube furnace under argon atmosphere for 6 h to obtain MnO2 powder.

[0097] (2) Grind the MnO2 powder to a particle size of 100-500 μm.

[0098] (3) Dissolve 123 mg ZrO2 calcined in step (2) in 300 mL deionized water and stir for 30 min, add 615 mg Cu(NO3)2•3H2O and 615 mg Sr(NO3)2•4H2O solid particles and stir for 2 h. Mix well, add 20 mg precipitant thiourea, stir at 80 °C for 8 h, precipitate at room temperature for 12 h, filter, wash, and dry at 90 °C for 10 h. Grind the obtained solid to 100-500 μm, and calcine at 500 °C in an argon atmosphere in a tube furnace for 4 h to obtain CuO-SrO / Mn 0.2 Zr 0.8 O2 composite oxygen carrier.

[0099] The oxygen carriers prepared in Examples 1 to 4 and Comparative Examples 1 to 5 were tested for average bulk density, average specific surface area, average pore volume, average pore diameter, and crushing strength. The test results are shown in Table 1.

[0100] The oxygen carrier prepared in Example 1 was applied according to Example 5, the oxygen carrier prepared in Example 2 was applied according to Example 6, the oxygen carrier prepared in Example 3 was applied according to Example 7, the oxygen carrier prepared in Example 4 was applied according to Example 8, and Comparative Examples 1 to 5 were all applied according to Example 5. The decomposition results of NH3 are shown in Table 2.

[0101] After the oxygen carrier prepared in Example 4 was used according to Example 8, the oxygen carrier was treated and circulated 10 times according to the conditions of Example 8, and the decomposition results of NH3 were tested. The results are shown in Table 3. The conversion rate of NH3 and the yield of H2 are calculated by the formula: .

[0102] Table 1 Detection results of oxygen carriers

[0103]

[0104] Table 2 Oxygen carriers for NH3 decomposition results

[0105]

[0106] Table 3 Experimental results of Example 8 repeated 10 times

[0107]

[0108] As can be seen from Table 1, the average bulk density, average specific surface area, average pore volume and average pore size of the composite oxygen carrier prepared by the present invention are all relatively large, and the crushing strength is relatively large, and the catalytic performance of the prepared composite oxygen carrier is good. As can be seen from Table 2, when the composite oxygen carrier prepared by the present invention is applied to the decomposition of NH3, the decomposition conversion rate is high, the hydrogen yield is high, and the catalytic performance is strong. As can be seen from Table 3, the composite oxygen carrier prepared by the present invention can be recycled, and the catalytic performance of the composite oxygen carrier obtained by recycling is still better. Along with the increase of cycle number, NH3 conversion rate and H2 productivity are relatively stable.

Claims

1. A CuO-SrO / Mn x Zr 1-x O 2 Preparation method of composite oxygen carrier, Features: The following steps are involved: (1) Mn(NO 3 ) 2 6H 2 O and ZrO(NO 3 ) 2 ·2H 2 O is dissolved in water, and then the two solutions are mixed, the pH of the solution is adjusted to 7-9, stirred at room temperature, filtered, washed, dried, and calcined to obtain Mn x Zr 1-x O 2 Powder, x is 0.2, 0.4, 0.6, 0.8; (2) Mn x Zr 1-x O 2 The powder is ground to a particle size of 100-500 μm; (3) The Mn ground in step (2) x Zr 1-x O 2 Dissolve in water and add Cu(NO 3 ) 2 •3H 2 O and Sr(NO 3 ) 2 •4H 2 O, mix evenly, add precipitant, stir at 60-100℃ for 6-12h, let stand for precipitation, filter, wash, dry, grind the obtained solid to 100-500μm, calcine, and obtain CuO-SrO / Mn x Zr 1-x O 2 Composite oxygen carrier; Mn x Zr 1-x O 2 、Cu(NO 3 ) 2 •3H 2 O、Sr(NO 3 ) 2 •4H 2 The mass ratio of O is 1:5:5, 94.2:11.7:35.3, 1:1.5:2.5 or 1.5:1:

1.

2. CuO-SrO / Mn according to claim 1 x Zr 1-x O 2 Preparation method of composite oxygen carrier, Features: In step (1), pH is adjusted by using one of ammonia water, sodium hydroxide and potassium hydroxide, with a mass concentration of 25%-30%.

3. The CuO-SrO / Mn according to claim 1 x Zr 1-x O 2 Preparation method of composite oxygen carrier, Features: The drying temperature of step (1) is 60-100°C and the drying time is 8-16h.

4. The CuO-SrO / Mn according to claim 1 x Zr 1-x O 2 Preparation method of composite oxygen carrier, Features: The calcination atmosphere of step (1) is argon or helium, the calcination temperature is 650-850°C, and the calcination time is 4-8h.

5. The CuO-SrO / Mn according to claim 1 x Zr 1-x O 2 Preparation method of composite oxygen carrier, Features: The precipitant in step (3) is thiourea or urea, 20-200 mg of which is added to every 100-500 mL of water.

6. The CuO-SrO / Mn according to claim 1 x Zr 1-x O 2 Preparation method of composite oxygen carrier, Features: The drying temperature of step (3) is 60-100°C and the drying time is 8-16h.

7. The CuO-SrO / Mn according to claim 1 x Zr 1-x O 2 Preparation method of composite oxygen carrier, Features: The calcination atmosphere in step (3) is argon or helium. The calcination is carried out in a tubular furnace at a temperature of 450-650° C. for a time of 3-6 hours.

8. A CuO-SrO / Mn x Zr 1-x O 2 Composite oxygen carrier, Features: The CuO-SrO / Mn x Zr 1-x O 2 The composite oxygen carrier is prepared by the preparation method.

9. The CuO-SrO / Mn according to claim 8 x Zr 1-x O 2 Application of composite oxygen carriers, Features: The following steps are involved: a. Put CuO-SrO / Mn x Zr 1-x O 2 The composite oxygen carrier is added to the fixed bed reactor, and pre-treated with nitrogen at a flow rate of 100-250 mL / min for 30-50 min. The preheater is set at 100-400°C, the fixed bed reactor is set at a reaction temperature of 200-500°C, and the temperature is increased and heated. The reaction pressure is set to 0.3-1 MPa; b. Introduce ammonia gas, set the ammonia gas inlet flow rate to 50-60 mL / min, and obtain hydrogen gas as a gas phase product; c. After the reaction is completed, nitrogen is introduced to exhaust the H 2 , continue to introduce oxygen into the fixed bed, set the temperature of the fixed bed reactor to 300-550℃, and obtain CuO-SrO / Mn with restored lattice oxygen x Zr 1-x O 2 Composite oxygen carrier.