Preparation method and application of quinary nano high-entropy alloy catalyst
By preparing a five-element nanometer high-entropy alloy catalyst, the problem of insufficient hydrogen absorption and release of MgH2 is solved. The nano-scale high-entropy alloy powder is compounded with MgH2 through ball milling and sintering processes, which significantly improves the hydrogen absorption and release kinetic properties and is suitable for Solid state hydrogen storage.
Patent Information
- Application Number
- CN202410879853.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to increase the hydrogen absorption and release capacity of MgH2 with existing technology, and an efficient high-entropy alloy catalyst is urgently needed.
The preparation method of a five-element nanometer high-entropy alloy catalyst includes ball milling a combination of chromium powder, cobalt powder, iron powder, manganese powder and V, Cr, Mo or Cu at a specific molar ratio, and then sintering, mechanical crushing and wet methods Mechanical ball milling, argon protection and deionized water cleaning were used to prepare nanometer high-entropy alloy powder with excellent catalytic properties, and compounded with MgH2 for solid-state hydrogen storage.
The hydrogen absorption and release kinetic properties of MgH2 are significantly improved, and the excellent catalytic performance is suitable for solid-state hydrogen storage applications.
Smart Images

Figure CN118719086A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical engineering, and in particular relates to a preparation method of a five-element nano high-entropy alloy catalyst and an application thereof. Background Art
[0002] High entropy alloys, also known as multi-group principal element alloys, are composed of five or more metal elements and have four unique effects: high entropy effect, lattice distortion effect, hysteresis diffusion effect and cocktail effect. The synergistic effect of multiple mechanisms gives them ultra-high stability and performance adjustability, especially in electrical properties, where multiple elements work synergistically to provide adsorption sites in different ranges, which is extremely ideal for achieving multi-kinetic catalysis.
[0003] Chinese invention patent application CN117758296A discloses an application of a high entropy alloy catalyst and a preparation method thereof, wherein the preparation method of the high entropy alloy catalyst comprises the following steps: S01: dissolving five metal salts in a solvent and mixing them to obtain a metal precursor mixed solution; S02: adding a stabilizer to the metal precursor mixed solution and mixing them thoroughly, and adding a reducing agent and mixing them thoroughly; S03: placing the mixed solution in a microwave reactor, maintaining an inert atmosphere, heating with microwaves and keeping the temperature to perform microwave-assisted reduction, and washing, drying and collecting the product; S04: placing the obtained product in a corrosive environment for corrosion to obtain a high entropy alloy catalyst with micropores. The invention uses non-precious metals to replace platinum group precious metals to obtain a high-efficiency bifunctional catalyst with low precious metal loading.
[0004] China's authorized invention patent CN115635097B discloses a laser powder bed fused high entropy alloy composite material with stable cellular structure and its preparation method, laser powder bed fused alloy powder and carbide powder are mixed evenly, and a high entropy alloy composite material with stable cellular structure is prepared by laser powder bed fusion technology, and the prepared high entropy alloy composite material still has stable cellular structure after heat treatment at ≥1100℃. The yield strength of the composite material is ≥800 MPa, the tensile strength is ≥1000 MPa, and the hardness is ≥350 HV.
[0005] How to obtain a high entropy alloy catalyst that can increase the amount of hydrogen absorbed and released by MgH2 is still a technical problem that needs to be solved urgently by technicians in this field. Summary of the invention
[0006] Based on the above reasons, the present invention proposes a preparation method and application of a five-element nano high-entropy alloy catalyst. Specifically, in order to achieve the purpose of the present invention, the present invention adopts the following technical solution: One aspect of the present invention relates to a method for preparing a five-element nano high-entropy alloy catalyst, which comprises the following steps: (1) preparing chromium powder, cobalt powder, iron powder, manganese powder and M powder having a molar ratio of 0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1, wherein M is one or a combination of V, Cr, Mo or Cu, and ball milling the weighed metal powders under the protection of inert gas to obtain alloy powder; (2) Press the alloy powder into a cylinder, and sinter the pressed metal cylinder at a sintering temperature of 1000°C to 1300°C for 5h to 10h; during the sintering process, introduce argon gas for protection to prevent oxidation; (3) Mechanically crushing the sintered metal cylinder into powder, and passing it through a 300-mesh sieve to obtain high entropy alloy powder; (4) Pour the ball milling beads, ethanol and the high entropy alloy powder of step (3) into a ball milling jar, fill it with argon gas for protection, and perform wet mechanical ball milling at 300 rpm to 420 rpm for 20 h to 60 h to obtain a high entropy alloy solid-liquid mixture.
[0007] (5) The ball-milled high-entropy alloy solid-liquid mixture is centrifuged and cleaned 4 to 5 times with deionized water, and the centrifuged high-entropy alloy powder is vacuum dried at a drying temperature of 60°C to 80°C.
[0008] In a preferred embodiment of the present invention, the ball milling process of step (1) is to weigh stainless steel ball milling beads according to a ball-to-material ratio of (40-80): 1, wherein beads with a diameter of 16 mm account for 5-15wt%, beads with a diameter of 10 mm account for 15-25wt%, and beads with a diameter of 3-7 mm account for 60-80wt%, and the ball milling beads and metal powder are poured into a ball milling jar and filled with argon for protection, and mechanical mixing is performed at 250rpm-350rpm for 10h-40h. The present invention uses beads of different diameters for ball milling, which helps to have a larger specific surface area under appropriate weighting conditions to crush the alloy powder and reduce the size of the alloy particles.
[0009] In a preferred embodiment of the present invention, the pressing process of step (2) is to weigh 3g~5g of powder and pour it into a mold, and press it into a cylinder with a diameter of 10-20mm and a thickness of 2-4mm under a pressure of 30Mpa.
[0010] In a preferred embodiment of the present invention, the sintering process in step (3) is followed by cooling by furnace cooling.
[0011] In a preferred embodiment of the present invention, the ball milling process of step (4) is as follows: stainless steel ball milling beads are weighed according to a ball-to-material ratio of (60-120):1, wherein beads with a diameter of 16 mm account for 10-20 wt%, beads with a diameter of 10 mm account for 20-30 wt%, and beads with a diameter of 5 mm account for 50-70 wt%, and dispersant and high entropy alloy powder are added in a ratio of (5-10):1, and wet mechanical ball milling is performed at 300 rpm-420 rpm for 20 h-60 h.
[0012] Another aspect of the present invention also relates to a five-element nano high entropy alloy catalyst prepared by the above preparation method.
[0013] Another aspect of the present invention also relates to the application of the five-element nano high entropy alloy catalyst of the present invention, and the application refers to the application in solid-state hydrogen storage.
[0014] In a preferred embodiment of the present invention, the five-element nano high entropy alloy catalyst is composited with MgH2 and used to absorb and release hydrogen.
[0015] Beneficial Effects The five-element nano high-entropy alloy catalyst of the present invention has excellent catalytic performance, significantly improves the hydrogen absorption and desorption kinetics of MgH2, and can be effectively applied to solid-state hydrogen storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a picture of the finished product of NiMnFeCoV high entropy alloy after sintering obtained according to the method of Example 1 of the present invention.
[0017] Figure 2 This is the XRD of the NiMnFeCoV nano high entropy alloy powder obtained according to the method of Example 1 of the present invention.
[0018] Figure 3 This is a SEM of the sintered NiMnFeCoV high entropy alloy obtained according to the method of Example 1 of the present invention.
[0019] Figure 4 This is the EDS of the NiMnFeCoV nano high entropy alloy powder obtained according to the method of Example 1 of the present invention.
[0020] Figure 5 This is the TEM of the NiMnFeCoV nano high entropy alloy powder obtained according to the method of Example 1 of the present invention.
[0021] Figure 6 This is an EDS graph of NiMnFeCoV nano high entropy alloy powder composite MgH2 obtained according to the method of Example 1 of the present invention.
[0022] Figure 7This is a performance diagram of NiMnFeCoV nano high entropy alloy powder catalyzing MgH2 obtained according to the method of Example 1 of the present invention, (a) is the hydrogen absorption performance, and (b) is the hydrogen release performance. DETAILED DESCRIPTION
[0023] In order to further understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Unless otherwise specified, the reagents involved in the embodiments of the present invention are all commercially available products and can be purchased through commercial channels. Embodiment 1:
[0025] First, chromium powder, cobalt powder, iron powder, manganese powder and vanadium powder that have passed through a 200-mesh sieve are prepared in a molar ratio of 1:1:1:1:(0.9~1.1) (the particle size of the metal powder is about 75 microns). The purity of the metal powder is above 99.99%. The weighed metal powder is poured into a stainless steel ball mill. Stainless steel ball mill beads are weighed according to the ball-to-material ratio (40~80):1, of which beads with a diameter of 16mm account for 10%, beads with a diameter of 10mm account for 20%, and beads with a diameter of 5mm account for 70%. The ball mill beads and metal powder are poured into the ball mill and filled with argon gas for protection. Mechanical mixing is performed on a planetary ball mill at 250rpm~350rpm for 10h~40h. 3g~5g of the mixed alloy powder is weighed and poured into a mold. A powder tablet press is used to press the mixed alloy powder into a cylinder with a diameter of 15mm and a thickness of 3mm at a pressure of 30Mpa. The pressed metal cylindrical piece is placed in a quartz crucible and sintered in a tube furnace at a sintering temperature of 1000°C to 1300°C and a sintering time of 5h to 10h. During the sintering process, argon is introduced for protection to prevent oxidation. The cooling is performed by furnace cooling. The sintered metal cylindrical piece is mechanically crushed into powder and passed through a 300-mesh sieve. The five-element high entropy alloy powder currently obtained does not reach the nanometer level, so mechanical ball milling is still used to reduce the particle size of the high entropy alloy. When mechanical ball milling is performed without adding a dispersant, at a large rotation speed, a large ball-to-material ratio and a long time, the high entropy alloy powder is easily smashed on the inner wall of the ball mill, resulting in a low discharge rate and an insignificant improvement in the size of the high entropy alloy particles. The present invention adopts wet ball milling, and ethanol is selected as a dispersant. Stainless steel ball milling beads are weighed according to the ball-to-material ratio (60 to 120): 1, wherein beads with a diameter of 16 mm account for 15%, beads with a diameter of 10 mm account for 25%, and beads with a diameter of 5 mm account for 60%. Dispersant and high entropy alloy powder are added in a ratio of (5~10):1. Pour the ball milling beads, ethanol and high entropy alloy powder into the ball milling jar and fill it with argon for protection. Perform wet mechanical ball milling at 300rpm~420rpm on a planetary ball mill for 20h~60h. Pour the ball-milled high entropy alloy solid-liquid mixture into a centrifuge tube and wash it 4~5 times in a centrifuge with deionized water. The centrifuge speed is 10000 rpm and the centrifugation time is 10min. Place the centrifuged high entropy alloy powder in a vacuum drying oven and dry it for 2h at a drying temperature of 60℃~80℃. Embodiment 2:
[0026] The NiMnFeCoCr nano high entropy alloy catalyst was prepared by the same method as in Example 1. Embodiment 3:
[0027] The NiMnFeCoMo nano high entropy alloy catalyst was prepared by the same method as in Example 1. Embodiment 4:
[0028] The NiMnFeCoCu nano high entropy alloy catalyst was prepared by the same method as in Example 1. Embodiment 5:
[0029] The high entropy alloy catalyst prepared in Example 1-4 was compounded with MgH2 and its hydrogen absorption and desorption capacity was evaluated. The prepared nano high entropy alloy powder was ball-milled with magnesium hydride in a mass ratio of 1:9 under argon protection. The ball milling time was 10h and the ball-to-material ratio was 100:1. After compounding, the phase and surface morphology were analyzed by XRD and SEM, and then the saturated hydrogen absorption and desorption at different temperatures were tested using a PCT hydrogen storage tester. The test results are shown in Table 1. The saturated hydrogen absorption capacity of NiMnFeCoV+MgH2 at 320°C was 5.922 wt.%, and the saturated hydrogen desorption capacity was 5.667 wt.%. Compared with the hydrogen absorption capacity of MgH2 at 320°C of 5.102 wt.%, the hydrogen desorption capacity was 0.214 wt.%, which can be seen that the high entropy alloy of the present invention has excellent catalytic performance and significantly improves the hydrogen absorption and desorption kinetics of MgH2. Among them, NiMnFeCoCr and NiMnFeCoV have the best performance.
[0030] Table 1. Hydrogen absorption and desorption of nano high entropy alloy catalyst composite MgH2 at 180 min Catalyst type <![CDATA[MgH2]]> <![CDATA[NiMnFeCoCr+ MgH2]]> <![CDATA[NiMnFeCoMo+ MgH2]]> <![CDATA[NiMnFeCoCu+ MgH2]]> <![CDATA[NiMnFeCoV+ MgH2 <!-- 3 -->]]> Hydrogen absorption at 280℃ (wt.%) / 5.633 5.477 4.449 5.772 Hydrogen release at 280℃ (wt.%) / 4.277 3.924 4.350 4.417 Hydrogen absorption at 300℃ (wt.%) 4.753 5.638 5.487 4.676 5.782 Hydrogen release at 300℃ (wt.%) 0.095 5.486 5.290 4.355 5.122 Hydrogen absorption at 320℃ (wt.%) 5.102 5.680 5.424 4.763 5.922 Hydrogen release at 320℃ (wt.%) 0.214 5.559 5.367 4.673 5.667 Hydrogen absorption at 350℃ (wt.%) 5.716 5.598 5.497 4.852 5.878 Hydrogen release at 350℃ (wt.%) 0.224 5.571 5.417 4.704 5.707 The above describes the preferred embodiments of the present invention, which are however not intended to limit the present invention. A person skilled in the art may make improvements and changes to the embodiments disclosed herein without departing from the scope and spirit of the present invention.
Claims
1. A method for preparing a five-element nano high entropy alloy catalyst, comprising the following steps: (1) preparing chromium powder, cobalt powder, iron powder, manganese powder and M powder having passed a 200-mesh sieve in a molar ratio of 0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1, wherein M is one or a combination of V, Cr, Mo or Cu, and ball milling under inert gas protection to obtain alloy powder; (2) Pressing the alloy powder into a cylinder, sintering the pressed metal cylinder at a sintering temperature of 1000°C to 1300°C for a sintering time of 5h to 10h; introducing argon gas during the sintering process; (3) Mechanically crushing the sintered metal cylinder into powder, and passing it through a 300-mesh sieve to obtain high entropy alloy powder; (4) Pour the ball milling beads, ethanol and high entropy alloy powder into a ball milling jar and fill it with argon gas for protection, and perform wet mechanical ball milling at 300 rpm to 420 rpm for 20 h to 60 h to obtain a high entropy alloy solid-liquid mixture; (5) The high entropy alloy solid-liquid mixture is centrifuged and washed 4 to 5 times with deionized water, and then vacuum dried at a drying temperature of 60°C to 80°C.
2. The preparation method according to claim 1, characterized in that: The ball milling in step (1) is performed by weighing stainless steel ball milling beads according to a ball to material ratio of (40-80):1, wherein beads with a diameter of 16 mm account for 5-15 wt%, beads with a diameter of 10 mm account for 15-25 wt%, and beads with a diameter of 3-7 mm account for 60-80 wt%, pouring the ball milling beads and metal powder into a ball milling jar, filling it with argon for protection, and mechanically mixing at 250 rpm-350 rpm for 10 h-40 h.
3. The preparation method according to claim 1, characterized in that: The pressing in step (2) is to weigh 3g-5g of powder and pour it into a mold, and press it into a cylinder with a diameter of 10-20mm and a thickness of 2-4mm under a pressure of 30Mpa.
4. The preparation method according to claim 1, characterized in that: After the sintering in step (3), the sintering is cooled by furnace cooling.
5. The preparation method according to claim 1, characterized in that: The ball milling in step (4) is as follows: stainless steel ball milling beads are weighed according to a ball-to-material ratio of (60-120):1, wherein beads with a diameter of 16 mm account for 10-20wt%, beads with a diameter of 10 mm account for 20-30wt%, and beads with a diameter of 5 mm account for 50-70wt%, dispersant and high entropy alloy powder are added in a ratio of (5-10):1, and wet mechanical ball milling is performed at 300rpm-420rpm for 20h-60h.
6. A five-element nano high-entropy alloy catalyst prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the five-element nano high entropy alloy catalyst according to claim 6 in solid-state hydrogen storage.
8. The use according to claim 7, characterized in that: The five-element nano high entropy alloy catalyst is used to absorb and release hydrogen after being compounded with MgH2.
Citation Information
Patent Citations
Preparation method of nano high-entropy alloy block material
CN110042295A
Carbon-loaded high-entropy alloy composite magnesium-based hydrogen storage material and preparation method thereof
CN113912006A
High-strength high-entropy alloy binding phase nanoscale hard alloy and preparation method thereof
CN116356173A
Alloy nanoparticles, aggregate of alloy nanoparticles, catalyst, and method for producing alloy nanoparticles
WO2021020377A1
Cited By
Method for preparing rare earth high-entropy alloy catalyst and application thereof
CN119680567A
A method for preparing a rare earth high entropy alloy catalyst and its application
CN119680567B