High-activity modified molecular sieve catalyst, preparation method thereof and application of high-activity modified molecular sieve catalyst in preparation of cyclohexane

By modifying the molecular sieve catalyst with metal and urea, the Ni-CoOx/β-U catalyst is formed, which solves the complex problem of molecular sieve catalyst modification in the existing technology, achieves the effect of highly selective preparation of cyclohexane under mild conditions, and simplifies The catalyst preparation and use process is improved, and the service life and recycling convenience of the catalyst are improved.

CN118719132AActive Publication Date: 2024-10-01ANHUI CARBON XIN TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410790787.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-01
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

Existing molecular sieve catalyst modification methods are complicated and can easily lead to skeleton collapse. They cannot effectively improve the selectivity and yield of hydrodeoxygenation products under mild conditions, affecting the upgrading and quality improvement of lignin oil.

Method used

Using metal and urea modified molecular sieve catalysts, a Ni-CoOx/β-U catalyst is formed through a specific preparation method, and n-hexane is used as the reaction solvent to achieve highly selective preparation of cyclohexane under mild conditions.

Benefits of technology

It achieves high activity and high selectivity hydrodeoxygenation reaction, simplifies the catalyst preparation and use process, extends the catalyst life, and has low cost. The catalyst is magnetic and easy to recycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719132A_ABST
    Figure CN118719132A_ABST
Patent Text Reader

Abstract

The invention discloses a high-activity modified molecular sieve catalyst as well as a preparation method and application thereof in preparation of cyclohexane. The catalyst is prepared through a simple impregnation-calcination-reduction method, and urea is added in the impregnation process to modify the molecular sieve. The obtained high-activity modified molecular sieve catalyst takes guaiacol as a reaction substrate, and the influence of different reaction temperatures, reaction time, catalyst dosage and other conditions on the reaction performance of the catalyst is investigated. Experiments show that the modified molecular sieve catalyst can completely convert guaiacol within 40 minutes at 180 DEG C, the product is cyclohexane, and the selectivity can reach 100%. The preparation method of the catalyst is simple, the catalyst is low in price, high in activity and good in stability, and the molecular sieve modification method is mild and effective. In the catalytic reaction process, n-hexane is used as a solvent, the reaction condition is mild, the reaction time is short, the energy consumption is low, the product is pure, and the application prospect is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of molecular sieve catalyst preparation and biomass technology, and in particular to a high-activity modified molecular sieve catalyst and a preparation method thereof and application thereof in the preparation of cyclohexane. Background Art

[0002] Biomass energy is an important component of renewable energy and is expected to become a substitute for traditional fossil energy. The main components of biomass include cellulose, hemicellulose and lignin, of which lignin accounts for about 20% to 30%. Lignin is a three-dimensional amorphous polymer formed by random bonding of three phenylpropane structural units through CC bonds and CO bonds. Its unique chemical structure makes it a potential substitute for traditional aromatic resources. However, lignin oil obtained by lignin depolymerization contains a large amount of phenolic derivatives, resulting in high oxygen content, low calorific value, poor chemical stability, etc., which seriously affects its wide application. Therefore, converting phenolic compounds into chemically stable cycloalkanes by hydrodeoxygenation is the most attractive and effective method for bio-oil modification and is the key to achieving lignin oil quality improvement.

[0003] The compounds in lignin oil are mainly phenolic derivatives with guaiacol-based structures, among which guaiacol is one of the most representative phenolic compounds in lignin oil. At present, the research on lignin hydrodeoxygenation mainly selects typical model compounds for research, and guaiacol is a commonly used model compound. In the process of upgrading lignin oil, a suitable catalytic system can not only promote hydrodeoxygenation, but also inhibit the occurrence of side reactions, thereby improving the selectivity of hydrodeoxygenation products. Molecular sieve catalysts have rich pore structures and acid sites, and show significant catalytic performance in the process of biomass oil value-added. Factors such as its grain size, pore structure, silicon-aluminum ratio and acid distribution have a direct impact on the yield and selectivity of the target product. The reported molecular sieve acid washing and alkali washing modification methods have cumbersome and complicated treatment processes, long modification time, and are prone to cause molecular sieve skeleton collapse, which seriously damages the acidity and pore structure of the molecular sieve and cannot effectively improve the comprehensive utilization value of the molecular sieve. Therefore, it is a technical problem to be solved urgently to effectively modify the molecular sieve under mild conditions, improve the yield and selectivity of the hydrodeoxygenation product, extend the life of the molecular sieve, achieve the breaking of the characteristic chemical bonds of lignin under mild conditions, and strengthen the process of directional hydrodeoxygenation of lignin oil to prepare cycloalkanes. Summary of the invention

[0004] In view of the above-mentioned technical deficiencies, the present invention provides a highly active modified molecular sieve catalyst and a preparation method thereof and application thereof in the preparation of cyclohexane, wherein the catalyst has the advantages of excellent hydrodeoxygenation ability, high selectivity and low cost. For the hydrodeoxygenation reaction of guaiacol, n-hexane is used as the reaction solvent, and cyclohexane can be prepared with high selectivity under mild conditions, which has a good market prospect.

[0005] In order to solve the problems of the prior art, the technical solution adopted by the present invention is:

[0006] A method for preparing a highly active modified molecular sieve catalyst comprises the following steps:

[0007] (1) Weighing cobalt nitrate hexahydrate, nickel nitrate hexahydrate and urea, adding them to methanol, and stirring at room temperature until they are uniformly dispersed to obtain solution A, wherein the concentrations of the cobalt nitrate hexahydrate and the nickel nitrate hexahydrate are 5 to 7 mg / mL, and the concentration of the urea is 2 to 3 mg / mL;

[0008] (2) Weigh the pretreated β-type molecular sieve and add it to solution A to obtain solution B. The amount of the molecular sieve added is 12 to 13 mg / mL. 2 / Al 2 O 3 The molar ratio is 20 to 40;

[0009] (3) heating solution B to 50-60° C. under magnetic stirring at 200-300 r / min to obtain a suspension, and crystallizing the suspension at 50-60° C. for 12-13 h, and then crystallizing at 10-20° C. for 12-13 h;

[0010] (4) removing methanol from the crystallized solution in step (3) under vacuum heating conditions, drying the precipitate, grinding it into powder, and then calcining it at 500-600° C. for 2-4 hours; cooling it to 10-20° C. and introducing hydrogen for reduction to obtain a highly active modified molecular sieve catalyst, denoted as Ni-CoOx / β-U.

[0011] Preferably, the molar ratio of nickel nitrate hexahydrate to cobalt nitrate hexahydrate in step (1) is 1:1.

[0012] Preferably, the pretreatment in step (2) is to treat the β-type molecular sieve SiO 2 / Al 2 O 3 The mixture was placed in a muffle furnace under air atmosphere at 500-600°C and calcined for 3-6 hours at a heating rate of 5°C / min.

[0013] Preferably, in step (2), the SiO 2 / Al 2 O 3 The molar ratio is 25, and the specific surface area of ​​the molecular sieve is 640m 2 / g, the heating temperature of solution B in step (3) is 55°C.

[0014] Preferably, the heating rate of calcination in step (4) is 2-5°C / min, the flow rate of hydrogen is 40-80 mL / min, the temperature during reduction is 300-600°C, and the reduction time is 1-3 h.

[0015] It is further preferred that in step (4), the powder calcination temperature is 550° C., and the calcination time is 3 h; the reduction temperature is 350° C., and the reduction time is 2 h.

[0016] The high-activity modified molecular sieve catalyst prepared by any of the above preparation methods.

[0017] The high-activity modified molecular sieve catalyst prepared by the above preparation method is used in the preparation of cyclohexane.

[0018] Preferably, the reactants and the catalyst are added to the reactor in a mass ratio of 1-6:1, and then the reaction solvent is added. After sealing, nitrogen is introduced to replace the air in the reactor. After repeating the replacement three times, 0.5-1.0 MPa hydrogen is then introduced. The mass ratio of the reaction solvent to the reactants is 130-200:1, and the mass ratio of the reaction solvent to the catalyst is 660-825:1. The temperature of the reactor is set to 140-240°C, the reaction time is 10-120 min, and the reaction is cooled to room temperature after the reaction is completed. The gas in the reactor is collected and the product is filtered and separated to obtain cyclohexane.

[0019] Preferably, the reaction solvent is one of methanol, ethanol, isopropanol or n-hexane; the reactant is guaiacol; the reaction heating rate is 8-10°C / min, and the stirring speed is 200-300r / min.

[0020] Beneficial effects:

[0021] Compared with the prior art, the high-activity modified molecular sieve catalyst and its preparation method and application in the preparation of cyclohexane of the present invention have the following advantages:

[0022] 1. The preparation process of the high-activity modified molecular sieve catalyst of the present invention is simple and low-cost, and has high activity and selectivity;

[0023] 2. The present invention selects metal and urea to modify the molecular sieve catalyst, which not only effectively regulates its pore size distribution and exposes more active sites, but also has little effect on the crystal composition of the catalyst. It is a mild and effective modification method. The obtained catalyst Ni-CoOx / Hβ-U has magnetic properties and is easy to recycle, which provides great convenience for post-reaction treatment.

[0024] 3. The catalyst Ni-CoOx / Hβ-U of the present invention can not only realize the hydrodeoxygenation of guaiacol, a lignin model compound, to prepare cyclohexane, but also can realize the hydrodeoxygenation of phenolic compounds in simulated lignin oil and complex real lignin oil to prepare cycloalkanes, and the preparation process route is short, the reaction equipment and operation method are simple, the reaction conditions are mild, the reaction time is short, and the complete hydrodeoxygenation of guaiacol to produce cyclohexane can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is the XRD pattern of the modified molecular sieve catalyst prepared in Example 1 of the present invention;

[0026] Figure 2 is the N of different molecular sieve catalysts 2 - adsorption-desorption curve, (a) is N 2 - adsorption-desorption curve, (b) pore size distribution diagram;

[0027] Figure 3 This is a SEM image of the modified molecular sieve catalyst prepared in Example 1 of the present invention;

[0028] Figure 4 TEM images of the modified molecular sieve catalyst prepared in Example 1 of the present invention, wherein (a) is a TEM image of the Ni-CoOx / Hβ-U catalyst, and (b) is a metal particle size distribution obtained from the TEM image of the Ni-CoOx / Hβ-U catalyst;

[0029] Figure 5 NH is the modified molecular sieve catalyst prepared in Example 1 of the present invention. 3 -TPD graph;

[0030] Figure 6 This is a diagram showing the conversion of guaiacol catalyzed by the catalyst prepared in Example 1 of the present invention at different hydrogen pressures;

[0031] Figure 7 The catalyst prepared in Example 1 of the present invention is a graph showing the conversion of guaiacol at different reaction times;

[0032] Figure 8 This is a diagram of the biomimetic oil hydrodehydrogenation conversion in Example 6 of the present invention, wherein (a) is the reaction substrate and product, and (b) is the GC-MS diagram after the reaction;

[0033] Fig. 9 This is a diagram of the hydrodeoxygenation conversion of dealkalized lignin oil in Example 7 of the present invention, wherein (a) is the original lignin oil and the liquid products obtained at different reaction times, (b) is a GC-MS diagram of the original lignin oil composition, and (c) is a GC-MS diagram of the liquid product after 10 hours of reaction;

[0034] Fig.101 and 1 are diagrams of the catalyst magnetic recycling experiment in Example 8, (a) is a diagram of the catalyst magnetic recovery, and (b) is the conversion rate and product yield of guaiacol during the catalyst recycling experiment. DETAILED DESCRIPTION

[0035] The following will be combined with the accompanying drawings in the examples of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The following examples are provided for a better understanding of the present invention, and are not limited to the best implementation mode, and do not limit the content and protection scope of the present invention. Any product that is the same or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0036] If no specific experimental steps or conditions are specified in the examples, the conventional experimental operations or conditions described in the literature in the field can be followed. If the manufacturer of the reagents or instruments used is not indicated, they are all conventional reagent products that can be purchased commercially.

[0037] Example 1 Preparation of Ni-CoOx / Hβ-U Catalyst

[0038] Solution A was obtained by dissolving 0.4 mmol of nickel nitrate hexahydrate, 0.4 mmol of cobalt nitrate hexahydrate and 0.8 mmol of urea in 20 mL of methanol.

[0039] Weigh 0.25g Hβ molecular sieve SiO 2 / Al 2 O 3 (Hβ molecular sieve was purchased from Tianjin Nanhua Catalyst Co., Ltd., SiO 2 / Al 2 O 3 The molar ratio is 25, and the specific surface area of ​​the molecular sieve is 640m 2 / g) was heated to 550°C in a muffle furnace at a heating rate of 5°C / min, calcined for 5h, and then added to solution A to obtain solution B.

[0040] Solution B was heated to 60°C in a 100 mL beaker with magnetic stirring at 200 rpm and stirred for 12 h, and then stirred at 10-20°C for 12 h while maintaining the speed unchanged.

[0041] The crystallized solution was heated at 37°C and 200 MPa to remove methanol under vacuum conditions, and the precipitate was dried in a vacuum oven at 80°C for 2 h, then ground into powder; then placed in a muffle furnace and heated to 550°C at a heating rate of 5°C / min for 3 h; after cooling to 10-20°C, H 2The temperature was raised to 350°C at a heating rate of 5°C / min under a nitrogen atmosphere and maintained at this temperature for 2 h. The flow rate of hydrogen was 60 mL / min.

[0042] Comparative Example 1

[0043] The preparation method is similar to that of Example 1, except that only calcined Hβ molecular sieve (Hβ molecular sieve purchased from Tianjin Nanhua Catalyst Co., Ltd., SiO 2 / Al 2 O 3 The molar ratio is 25, and the specific surface area of ​​the molecular sieve is 640m 2 / g) and urea, and the product was recorded as Hβ-U catalyst.

[0044] Comparative Example 2

[0045] The preparation method is similar to that of Example 1, except that urea is not added to solution A, and only nickel nitrate hexahydrate and cobalt nitrate hexahydrate are added. The product is recorded as Ni-CoOx / Hβ catalyst.

[0046] Comparative Example 3

[0047] The preparation method is similar to that of Example 1, except that cobalt nitrate hexahydrate is not added to solution A, and only nickel nitrate hexahydrate and urea are added. The product is recorded as Ni / Hβ-U bimetallic catalyst.

[0048] Comparative Example 4

[0049] The preparation method is similar to that of Example 1, except that nickel nitrate hexahydrate is not added to solution A, and only cobalt nitrate hexahydrate and urea are added. The product is recorded as CoOx / Hβ-U catalyst.

[0050] Figure 1 The X-ray diffraction patterns of the catalysts prepared in Example 1 and Comparative Examples 1-4 are shown in FIG. As can be seen from the figure, characteristic absorption peaks of β molecular sieve appear at 7.93°, 22.49°, 25.34°, 27.08° and 29.66°, and the XRD spectra of the catalysts modified with urea and unmodified are basically the same, indicating that the process of modifying the molecular sieve with urea does not damage the crystal structure of the molecular sieve, which indicates that the method of modifying the molecular sieve with urea is a relatively mild treatment method. The peaks at 36.49°, 42.38° and 61.49° belong to the (111), (200) and (220) crystal planes of CoO, respectively, and the peaks at 37.28°, 43.27° and 62.87° belong to the (111), (200) and (220) crystal planes of NiO, respectively. Since the diffraction peaks of CoO and NiO are in similar positions, the main diffraction peaks in Ni-CoOx / Hβ-U and Ni-CoOx / Hβ catalysts are NiO, CoO or their composites.

[0051] Figure 2 N is the N of the catalysts prepared in Example 1 and Comparative Example 2 of the present invention. 2 -Adsorption-desorption curves. According to the IUPAC classification, both Ni-CoOx / Hβ-U and Ni-CoOx / Hβ catalysts exhibit type IV isotherms and H2-type hysteresis loops, indicating that the mesoporous structure is dominant in these materials. From the characterization results, it can be seen that after the addition of urea, the hysteresis loop is distorted and gradually moves toward the high-pressure direction, and some ordered mesopores in the catalyst are destroyed. The specific surface area of ​​the Ni-CoOx / Hβ-U catalyst measured by the BET method is 480.596m 2 / g, pore volume 373.93cm 3 / g, its specific surface area and pore volume are better than those of the unmodified Ni-CoOx / Hβ catalyst, which indicates that the larger specific surface area and pore volume make Ni-CoOx / Hβ-U have better hydrodeoxygenation catalytic performance.

[0052] Figure 3 This is a scanning electron microscope spectrum of the Ni-CoOx / Hβ-U catalyst prepared in Example 1. It can be clearly seen from the figure that the surface morphology of the Ni-CoOx / Hβ-U catalyst is rough, with regularly stacked grains, indicating that the metal and urea modification methods retain the complete pore structure of the β-type molecular sieve. From the EDS surface spectrum of the Ni-CoOx / Hβ-U catalyst, it can be seen that the Ni and Co elements are uniformly dispersed on the carrier, and no peaks of other elements are detected in the surface spectrum, indicating that the catalyst prepared by the present invention is relatively pure.

[0053] Figure 4 This is a transmission electron microscope TEM image of the Ni-CoOx / Hβ-U catalyst prepared in Example 1. It can be seen from the figure that the metal active particles are evenly dispersed and small in size, with an average size of 3.43nm. The smaller the particle size, the easier it is to activate hydrogen to contact the substrate during the reaction, thereby showing better catalytic performance. Among them, (a) is a TEM image of the Ni-CoOx / Hβ-U catalyst, and (b) is the metal particle size distribution obtained from the TEM image of the Ni-CoOx / Hβ-U catalyst.

[0054] 50 mg of Ni-CoOx / Hβ-U prepared in Example 1 and Ni-CoOx / Hβ catalyst prepared in Comparative Example 1 were respectively taken and pretreated at 250°C for 2 h in an Ar atmosphere, cooled to 100°C, and then NH 3 The adsorption was saturated, and then the physically adsorbed NH 3 Finally, the temperature was raised to 700℃ at 10℃ / min for programmed temperature desorption. Figure 5As shown. It can be seen from the figure that the peak below 250℃ corresponds to the weak acid site of the catalyst; the peak between 250℃ and 420℃ corresponds to the medium-strong acid site of the catalyst, and the peak between 420℃ and 550℃ corresponds to the strong acid site of the catalyst. In addition, the catalyst has medium-strong acid and strong acid sites, among which the content of strong acid sites on the surface of the molecular sieve catalyst modified by urea decreases, and the content of weak acid sites increases. This may be because the weak base generated by urea during the thermal decomposition process of urea is desiliconized, and part of the non-framework aluminum is inserted into the molecular sieve framework, resulting in a decrease in strong acid sites.

[0055] Example 2 After guaiacol hydrodeoxygenation reaction

[0056] 60 mg of guaiacol, 20 mg of catalyst and 20 mL of n-hexane solvent were added to a high-pressure reactor, which was sealed and nitrogen was introduced to replace the air in the reactor. After the replacement was repeated 3 times, 1 MPa of hydrogen was then introduced.

[0057] The temperature was raised to 140-200°C at a heating rate of 10°C / min, and the reaction was carried out at a rotation speed of 300r / min for 10-120min. After the reaction, the high-pressure reactor was cooled to room temperature, the gas in the reactor was collected, the catalyst was filtered and separated, and the product distribution was characterized and analyzed by GC-MS.

[0058] Example 3 Effect of different catalysts on the hydrodeoxygenation of guaiacol

[0059] Reaction conditions: 60 mg guaiacol, 20 mg catalyst, 20 mL n-hexane, 180 °C, 1 MPa H 2 , 2h.

[0060] Table 1 shows the effect of different catalysts on the hydrodeoxygenation of guaiacol

[0061]

[0062] As can be seen from Table 1, when only the β-type molecular sieve support was used to catalyze the conversion of guaiacol, no reaction occurred. When the support was loaded with metal Ni or Co oxides, guaiacol began to be converted, mainly producing cyclohexane, which indicates that the metal-modified molecular sieve can provide active reaction centers for the hydrodeoxygenation reaction of guaiacol and catalyze the hydrodeoxygenation conversion of guaiacol.

[0063] Only metal-modified molecular sieve catalysts were used, and molecular sieve catalysts without urea modification were able to catalyze the conversion of guaiacol, with a conversion rate of 92.88%. Four products were obtained, and the selectivity of the main product cyclohexane was low (high selectivity means that the only product produced after the reaction was cyclohexane). Ni-CoOx / Hβ-U modified with urea showed the best catalytic performance. Under the conditions of a reaction temperature of 180°C and n-hexane as a solvent, it was able to catalyze the complete conversion of guaiacol, and the only product was cyclohexane, indicating that the prepared Ni-CoOx / Hβ-U catalyst effectively catalyzed the hydrodeoxygenation of guaiacol to cyclohexane.

[0064] Example 4 Effect of reaction hydrogen pressure on guaiacol hydrodeoxygenation

[0065] Reaction conditions: 60 mg guaiacol, 20 mg catalyst prepared in Example 1, 20 mL n-hexane, 180° C., 2 h.

[0066] Figure 6 The effect of different hydrogen pressures on the catalytic conversion of guaiacol. When the hydrogen pressure is 0.5MPa, the conversion rate of guaiacol is 67.64%, and the only product is cyclohexane. As the pressure increases from 0.5MPa to 1MPa, the conversion rate of guaiacol reaches 100%, and the yield of cyclohexanol is 100%, which shows that increasing the hydrogen pressure can promote the hydrodeoxygenation of guaiacol to produce cyclohexane. As the hydrogen pressure is further increased to 2MPa, the conversion rate of guaiacol and the yield of cyclohexane are basically unchanged.

[0067] From the perspective of practical application, considering the economic cost, hydrogen resources must be used rationally and fully utilized. Therefore, a hydrogen pressure of 1 MPa is selected as the optimal reaction pressure for this reaction system.

[0068] Example 5 Effect of reaction time on guaiacol hydrodeoxygenation

[0069] Reaction conditions: 60 mg guaiacol, 20 mg catalyst prepared in Example 1, 20 mL n-hexane, 180 °C, 1 MPaH 2 .

[0070] Figure 7The effect of different reaction times on the catalytic conversion of guaiacol. When the reaction time is 10 min, the conversion rate of guaiacol is 13.12%, and the only product is cyclohexane. As the reaction time is extended to 20 min, the conversion rate of guaiacol increases to 59.91%, and the product contains cyclohexane with a yield of 51.18%, cyclohexanol with a yield of 3.45%, trans-1,2-cyclohexanediol with a yield of 1.74%, and cyclohexanediol with a yield of 3.42%. Continue to extend the reaction time, the conversion rate of guaiacol increases. When the reaction is 40 min, the conversion rate of guaiacol reaches 100%, the yield of cyclohexane is 100%, and the selectivity is 100%, which shows that extending the reaction time can not only improve the conversion rate of guaiacol, but also promote the further hydrodeoxygenation of the intermediate product to produce cyclohexane. As the reaction time was further extended to 60 min, the conversion rate of guaiacol and the yield of cyclohexane remained basically unchanged, which indicates that the catalyst can catalyze the highly selective conversion of guaiacol into cyclohexane under mild conditions and has high activity.

[0071] Example 6: Hydrodeoxygenation of simulated lignin oil (imitation wood oil)

[0072] Reaction conditions: 60 mg of guaiacol (conventional commercial product), 4-methylanisole, m-cresol, 2,6-dimethoxy-4-methylphenol and 2-methoxy-4-propylphenol mixture, 20 mg of the catalyst prepared in Example 1, 20 mL of n-hexane, 180°C, 1 MPa H 2 .

[0073] Figure 8 This is a diagram of the hydrodeoxygenation reaction of simulated lignin oil catalyzed by Ni-CoOx / Hβ-U catalyst. Real lignin oil is usually a mixture of multiple compounds. After roughly understanding the catalytic hydrodeoxygenation reaction mechanism through a single reactant, five compounds with high content in lignin oil (guaiacol, 4-methylanisole, m-cresol, 2,6-dimethoxy-4-methylphenol and 2-methoxy-4-propylphenol) were mixed to prepare simulated oil. It can be seen from the figure that only cyclohexane, methylcyclohexane and propylcyclohexane were detected in the products after the reaction, which shows that Ni-CoOx / Hβ-U catalyst can effectively catalyze the hydrodeoxygenation of simulated wood oil to produce cycloalkane compounds.

[0074] Example 7 Hydrodeoxygenation of dealkalized lignin oil

[0075] Reaction conditions: 60 mg of dealkalized lignin oil (dealkalized lignin oil is obtained by alcoholysis of commercially available industrial dealkalized lignin in isopropanol at 300°C for 4 h, wherein the dealkalized lignin concentration is 4 mg / mL), 20 mg of the catalyst prepared in Example 1, 20 mL of n-hexane, 200°C, 1 MPa H 2 .

[0076] Fig. 9 This is the GC-MS gas chromatography-mass spectra of the Ni-CoOx / Hβ-U catalyst before and after the hydrodeoxygenation reaction of dealkalized lignin oil. It can be seen from the figure that as the reaction time increases, the color of the lignin oil after the reaction gradually becomes lighter. When the reaction is continued for 10 hours, the product is almost colorless. By comparing the gas chromatography-mass spectra of the dealkalized lignin oil and the product after 10 hours of reaction, it can be seen that a large number of cycloalkane compounds were detected in the dealkalized lignin oil after the reaction, and the hydroxyl and methoxy groups in most of the compounds in the original lignin oil were removed, indicating that the Ni-CoOx / Hβ-U catalyst can effectively achieve the hydrodeoxygenation of complex lignin oil under mild conditions.

[0077] Example 8 Catalyst recovery cycle experiment

[0078] Reaction conditions: 60 mg of guaiacol, 20 mg of the catalyst prepared in Example 1, 20 mL of n-hexane, 180°C, 40 min, 1 MPaH 2 .

[0079] Fig.10 This is a recycling experiment diagram of the Ni-CoOx / Hβ-U catalyst. It can be seen from the figure that the prepared catalyst has magnetic properties and can be separated, recycled and reused using an external magnetic field during the recycling process. In addition, after the catalyst was recycled 5 times, the conversion rate of guaiacol decreased, while the selectivity of cyclohexane in the product was still 100%, which shows that the Ni-CoOx / Hβ-U catalyst has good recycling stability.

[0080] In summary, the metal and urea modified molecular sieve catalyst used in the present invention not only effectively regulates its pore size distribution and exposes more active sites, but also has little effect on the crystal composition of the catalyst. It is a mild and effective modification method. The obtained catalyst Ni-CoOx / Hβ-U has magnetic properties and is easy to recycle, which provides great convenience for post-reaction treatment. In addition, the present invention uses a catalyst containing aromatic rings and C ar -OH and C ar -OCH 3 Guaiacol containing oxygen functional groups is used as a model compound of lignin. By optimizing the reaction conditions, the molecular sieve catalyst is modified from the perspective of practical application. Under low temperature and short reaction time conditions, guaiacol can be highly selectively hydrodeoxygenated to cyclohexane.

[0081] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a high-activity modified molecular sieve catalyst, characterized in that: The following steps are involved: (1) Weighing cobalt nitrate hexahydrate, nickel nitrate hexahydrate and urea, adding them to methanol, and stirring at room temperature until they are uniformly dispersed to obtain solution A, wherein the concentrations of the cobalt nitrate hexahydrate and the nickel nitrate hexahydrate are 5 to 7 mg / mL, and the concentration of the urea is 2 to 3 mg / mL; (2) Weighing the pretreated β-type molecular sieve and adding it to solution A to obtain solution B, wherein the amount of the molecular sieve added is 12 to 13 mg / mL, wherein the molar ratio of SiO2 / Al2O3 in the β-type molecular sieve is 20 to 40; (3) heating solution B to 50-60° C. under magnetic stirring at 200-300 r / min to obtain a suspension, and crystallizing the suspension at 50-60° C. for 12-13 h, and then crystallizing at 10-20° C. for 12-13 h; (4) removing methanol from the crystallized solution in step (3) under vacuum heating conditions, drying the precipitate, grinding it into powder, and then calcining it at 500-600° C. for 2-4 hours; cooling it to 10-20° C. and introducing hydrogen for reduction to obtain a highly active modified molecular sieve catalyst, denoted as Ni-CoOx / β-U.

2. The method for preparing a highly active modified molecular sieve catalyst according to claim 1, characterized in that: The molar ratio of nickel nitrate hexahydrate to cobalt nitrate hexahydrate in step (1) is 1:

1.

3. The method for preparing a highly active modified molecular sieve catalyst according to claim 1, characterized in that: The pretreatment in step (2) is to place the β-type molecular sieve SiO2 / Al2O3 in a muffle furnace in an air atmosphere at 500-600°C for calcination for 3-6 hours at a heating rate of 5°C / min.

4. The method for preparing a highly active modified molecular sieve catalyst according to claim 1, characterized in that: In step (2), the molar ratio of SiO2 / Al2O3 in the molecular sieve is 25, and the specific surface area of ​​the molecular sieve is 640m 2 / g, the heating temperature of solution B in step (3) is 55°C.

5. The method for preparing a highly active modified molecular sieve catalyst according to claim 1, characterized in that: In step (4), the heating rate of calcination is 2-5°C / min, the flow rate of hydrogen is 40-80mL / min, the temperature during reduction is 300-600°C, and the reduction time is 1-3h.

6. The method for preparing a highly active modified molecular sieve catalyst according to claim 5, characterized in that: In step (4), the powder calcination temperature is 550° C. and the calcination time is 3 h; the reduction temperature is 350° C. and the reduction time is 2 h.

7. A high-activity modified molecular sieve catalyst prepared by any one of the preparation methods described in claims 1-6.

8. Use of the high-activity modified molecular sieve catalyst prepared by the preparation method according to claim 1 in the preparation of cyclohexane.

9. The use according to claim 7, characterized in that: The reactants and the catalyst are added into the reactor in a mass ratio of 1-6:1, and then the reaction solvent is added. After sealing, nitrogen is introduced to replace the air in the reactor. After repeating the replacement 3 times, 0.5-1.0 MPa hydrogen is introduced. The mass ratio of the reaction solvent to the reactants is 130-200:1, and the mass ratio of the reaction solvent to the catalyst is 660-825:

1. The temperature of the reactor is set at 140-240°C, the reaction time is 10-120 min, and after the reaction is completed, it is cooled to room temperature, the gas in the reactor is collected, and the product is separated by filtration to obtain cyclohexane.

10. The use according to claim 9, characterized in that: The reaction solvent is one of methanol, ethanol, isopropanol or n-hexane; the reactant is guaiacol; the reaction heating rate is 8-10°C / min, and the stirring speed is 200-300r / min.

Citation Information

Patent Citations

  • Catalyst of hydrodeoxygenation reaction and its preparation method and application

    CN107649169A

  • Nickel cobalt oxide catalyst used for hydrolysis of sodium borohydride and preparation method of catalyst

    CN108380238A

  • Preparation of magnetic bifunctional catalyst NiCoAl and research method for hydrodeoxygenation of lignin phenol derivative

    CN116265088A

  • Preparation method of NiCo / MCM-41 catalyst for lignin derivative conversion