Application and method for separating injection-molded part / glued part by using nano bubble solution

Through the application of nanobubble solution, the mechanical and charge effects of nanobubbles are used to solve the problem of separation of injection molded parts and adhesive joints in waste electronic equipment, achieve efficient and environmentally friendly recycling, and avoid the environmental pollution problems of traditional methods.

CN118719781APending Publication Date: 2024-10-01EAST CHINA UNIV OF SCI & TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410879178.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to effectively separate and recycle injection molded parts and adhesive parts in waste electronic equipment with existing technology, and the traditional method uses volatile solvents, which causes greater environmental pollution.

Method used

Nanobubble solution is used for separation. By controlling the particle size and Zeta potential of nanobubbles, mechanical stirring, sonic vibration and other methods are used to prepare the nanobubble solution. It combines heating and stirring to process waste electronic equipment to achieve efficient removal of injection molded parts and glued joints. Plasticizing and degumming.

Benefits of technology

It achieves efficient separation without volatile solvents, reduces environmental pollution, is economical, and is suitable for batch processing of different types of waste electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719781A_ABST
    Figure CN118719781A_ABST
Patent Text Reader

Abstract

The invention discloses a method for separating an injection-molded part / glue-connected part by using a nano-bubble solution, which comprises the following steps of: soaking a device to be treated in the nano-bubble solution, and heating and stirring in the soaking process; wherein the to-be-processed device and the nano bubble solution have charges with opposite electrical properties; the absolute value of the Zeta potential of the nano bubble solution is not less than 25mV; in the nano bubble solution, the average particle size of nano bubbles does not exceed 200nm. The invention also discloses an application of the nano-bubble solution in recovery of waste electronic equipment. Compared with a traditional recycling method, the method for separating the injection molding part / glue connecting part through the nanometer bubble solution only needs energy, water and air, a series of different types of waste electronic products can be treated in batches, and effective plastic removal and glue removal of a base material can be achieved in a green and efficient mode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of post-processing of waste electronic equipment, and in particular to an application and method of separating injection molded parts / adhesive joints by using a nano bubble solution. Background Art

[0002] With the popularization of electronic products and the accelerated pace of replacement, a large number of waste electronic equipment are generated, which has caused a series of problems for environmental protection and resource management. At the same time, waste electronic equipment contains rich resources, including metals, precious metals, plastics, glass and rare elements, etc. These resources can be reprocessed to produce new electronic products or other industrial applications. In order to achieve the effects of thinness, waterproofness and other effects of electronic products, a large number of injection molded parts and adhesive parts are used in electronic products. The use of these connection methods has brought a series of problems to the post-processing of electronic products. First, the metal containing injection molded parts cannot be directly recycled because plastics will affect the smelting process; secondly, injection molded parts are difficult to remove, and volatile non-polar / polar solvents are generally used, which are easy to affect the environment.

[0003] In view of the current research difficulties in separating injection molded parts and glued parts in discarded electronic equipment, it is urgent to develop a cost-effective, green and universal process. Summary of the invention

[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide an application and method for separating injection molded parts / adhesive parts using nanobubble solution. Compared with traditional recycling methods, the method of the present invention only requires energy, water and air, and can process a series of different types of waste electronic products in batches, and can effectively deplasticize and debond the matrix material in an environmentally friendly and efficient manner.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] In a first aspect, the present invention provides the use of a nanobubble solution in separating injection molded parts / adhesive parts.

[0007] In the present invention, nanobubble solution refers to a liquid system mixed with nanobubbles, and such liquid systems include aqueous solutions, aqueous solutions, and the like.

[0008] In some exemplary embodiments of the present invention, in the nanobubble solution, the average particle size of the nanobubbles is no more than 200 nm, for example no more than 150 nm, no more than 100 nm, no more than 50 nm; for example, 1 nm to 50 nm, for example, 1 nm to 40 nm, for example, 1 nm to 30 nm, for example, 3 nm to 30 nm, for example, 5 nm to 30 nm, for example, 8 nm to 30 nm, for example, 10 nm to 30 nm, for example, 10 nm to 25 nm, for example, 10 nm to 20 nm, for example, about 10 nm, for example, about 11 nm, for example, about 12 nm, for example, about 13 nm, for example, about 14 nm, for example, about 15 nm, for example, about 16 nm, for example, about 17 nm, for example, about 18 nm, for example, about 19 nm, for example, about 20 nm, etc., but is not limited to the listed values, and other unlisted values ​​or ranges within the numerical range are equally applicable.

[0009] The term "average particle size" used in this article refers to the D50 particle size of nanobubbles, that is, the particle size corresponding to when the cumulative particle size distribution percentage of nanobubbles in the solution reaches 50%. Its physical meaning is that bubbles with a particle size larger than it account for 50%, and bubbles with a particle size smaller than it also account for 50%. D50 is also called the median diameter or median particle size, and is often used to indicate the average particle size of a powder.

[0010] In some exemplary embodiments of the present invention, the absolute value of the zeta potential of the nanobubble solution is not less than 25 mV; for example, not less than 30 mV, not less than 40 mV, not less than 50 mV, not less than 60 mV. Optionally, the absolute value of the zeta potential of the nanobubble solution is between 25 mV and 100 mV, preferably 30 mV to 100 mV, preferably 30 mV to 80 mV, preferably 40 mV to 80 mV. As an example, the absolute value of the zeta potential of the nanobubble solution can be about 40mV, 41mV, 42mV, 43mV, 44mV, 45mV, 46mV, 47mV, 48mV, 49mV, 50mV, 51mV, 52mV, 53mV, 54mV, 55mV, 56mV, 57mV, 58mV, 59mV, 60mV, 61mV, 62mV, 63mV, 64mV, 65mV, 66mV, 67mV, 68mV, 69mV, 70mV, 71mV, 72mV, 73mV, 74mV, 75mV, 76mV, 77mV, 78mV, 79mV, 80mV, etc., but is not limited to the listed values, and other values ​​or ranges not listed within the numerical range are also applicable.

[0011] The term "Zeta potential" as used herein refers to the potential of the shear plane, also known as the electrokinetic potential or electromotive force (ζ-potential or ζ-potential). The higher the absolute value (positive or negative) of the Zeta potential, the more stable the system, i.e., the dissolution or dispersion can resist aggregation. Conversely, the lower the absolute value (positive or negative) of the Zeta potential, the more prone to agglomeration or coagulation.

[0012] In the present invention, the nano bubble solution can be prepared by a variety of methods. For example, in some exemplary embodiments of the present invention, the preparation method of the nano bubble solution includes mechanical stirring, acoustic vibration, electrolysis, atomization, hydrodynamic cavitation, optical cavitation, etc. The time for treating the liquid using the bubble generation method can be at least 30 seconds, preferably 30 seconds to 60 minutes, such as 1 minute to 60 minutes, 1 minute to 55 minutes, 1 minute to 50 minutes, 1 minute to 45 minutes, 1 minute to 40 minutes, 1 minute to 35 minutes, 1 minute to 30 minutes, 2 minutes to 30 minutes, 3 minutes to 30 minutes, 4 minutes to 30 minutes, 5 minutes to 30 minutes.

[0013] In some preferred embodiments of the present invention, the bubble generation method is mechanical stirring. During high-speed stirring, shear force helps to generate smaller and more uniform nanobubbles; the faster the stirring speed, the smaller the particle size of the generated nanobubbles; conversely, the slower the stirring speed, the larger the particle size of the generated nanobubbles. Therefore, by adjusting the stirring speed, the particle size of the generated nanobubbles can be regulated. This method has been described in detail in Chinese patent CN117339411A, and will not be repeated here.

[0014] In some preferred embodiments of the present invention, when mechanical stirring is used to prepare nanobubbles, a stirring device is provided in the container for stirring the liquid (e.g., water). Specifically, the stirring speed of the stirring device can be 100 rpm to 10000 rpm, such as about 200 rpm, about 300 rpm, about 400 rpm, about 500 rpm, about 600 rpm, about 700 rpm, about 800 rpm, about 900 rpm, about 1000 rpm, about 2000 rpm, about 3000 rpm, about 4000 rpm, about 5000 rpm, about 6000 rpm, about 7000 rpm, about 8000 rpm, about 9000 rpm, etc., but are not limited to the listed values, and other unlisted values ​​or ranges within the numerical range are also applicable. After rapid mechanical stirring, the nanobubbles will enter and stably exist in the solution system.

[0015] In some preferred embodiments of the present invention, the concentration of nanobubbles contained in the nanobubble solution is at least about 1.0×10 10(pcs) / mL, for example, the concentration of nanobubbles contained in the nanobubble solution is about 1.0×10 10 (pcs) / mL to about 1.0×10 11 (pcs) / mL, e.g. 5.0×10 10 (pcs) / mL to about 1.0×10 11 (pieces) / mL.

[0016] In some exemplary embodiments of the present invention, the gas in the nanobubble can be not only a single gas component, but also a mixed gas composed of several gas components. As an exemplary embodiment, the gas in the nanobubble can include one or more of air, nitrogen (N2), oxygen (O2), carbon dioxide (CO2), ozone (O3), nitric oxide (NO), nitrogen dioxide (NO2), helium (He) gas, neon (Ne) gas, argon (Ar) gas and the like. In a preferred embodiment, the gas in the nanobubble includes oxygen. In some preferred embodiments, the gas in the nanobubble is oxygen. In other preferred embodiments, the gas in the nanobubble contains oxygen and other gases, such as air.

[0017] In the present invention, the Zeta potential of the nanobubble solution can be regulated by various known methods. For example, in some exemplary embodiments, in the process of preparing nanobubbles, the Zeta potential of the nanobubble solution can be changed by adjusting the pH value of the liquid, adding specific electrolytes to the liquid, etc. For example, in some embodiments, a certain amount of cationic surfactant is added to the liquid to obtain a nanobubble solution with a positive Zeta potential. In other embodiments, a certain amount of anionic surfactant is added to the liquid to obtain a nanobubble solution with a negative Zeta potential.

[0018] In a second aspect, the present invention also provides the use of the nanobubble solution in the recycling of waste electronic equipment.

[0019] Plastic parts, adhesive parts and other components are widely used in waste electronic equipment. It is difficult to separate these plastic parts, adhesive parts and recyclable parts such as metal parts and screens using ordinary processing methods. Based on the characteristics of nanobubble solution that can efficiently separate injection molded parts / adhesive parts, it is applied to the recycling of waste electronic equipment to achieve efficient plastic and adhesive removal of recyclable parts in waste electronic equipment.

[0020] In a third aspect, the present invention also provides a method for separating injection molded parts / adhesive parts using a nanobubble solution, comprising:

[0021] placing the device to be processed in a nanobubble solution for immersion, wherein heating and stirring are performed during the immersion process;

[0022] The device to be processed and the nanobubble solution have charges of opposite electrical properties; the absolute value of the Zeta potential of the nanobubble solution is not less than 25 mV; and the average particle size of the nanobubbles in the nanobubble solution does not exceed 200 nm.

[0023] In the present invention, the device to be processed can be any device containing injection molded parts and / or adhesive parts, preferably waste electronic equipment. In some exemplary embodiments of the present invention, the waste electronic equipment can be a computer, a mobile phone, a tablet, an earphone, an electronic watch, etc.

[0024] Nanobubbles have many excellent properties, such as long residence time in solution, high mass transfer efficiency and large specific surface area, which make them have broad application prospects in many fields. In the present invention, the inventor creatively uses nanobubble solution in the recycling of waste electronic equipment. The unique properties of nanobubbles make them play a vital role in the separation process of injection molded parts / adhesive parts and matrix materials. Specifically, the role of nanobubbles in the separation of waste electronic equipment can be described in detail from the following aspects:

[0025] (1) Separation effect under high temperature conditions: During the processing, waste electronic equipment will be heated to a certain high temperature, which helps soften the injection molded parts and adhesive parts, making them more susceptible to external forces. The particle size of nanobubbles is usually between a few nanometers and a few hundred nanometers. The particle size is small and the density is low. Under high temperature, they will show more active irregular motion. These high-speed nanobubbles constantly hit the surfaces of injection molded parts and adhesive parts, generating mechanical forces, which helps to destroy the structure of these materials and gradually loosen them.

[0026] (2) Generation of shock waves and the role of hydroxyl radicals: During the impact process, nanobubbles will burst due to excessive force. When bursting, the gas in the nanobubbles is rapidly released, generating high-energy shock waves in a short period of time. These shock waves act on injection molded parts and adhesive parts, further destroying their structure and the bonding force between molecules. At the same time, after the nanobubbles burst, a large number of hydroxyl radicals (·OH) with strong oxidizing properties will be generated in the solution, which can oxidize the organic molecules in the injection molded parts and adhesive parts, destroy their chemical bonds, especially the connection between polymer chains, and further weaken their structural stability.

[0027] (3) Charged suction: Nanobubbles can be charged with a specific charge (positive or negative) on their surface by adjusting the pH value of the solution or adding specific electrolytes. A large number of nanobubbles with a specific charge will generate a huge charged suction in the solution. This suction can target injection molded parts and adhesive parts, thereby effectively weakening the bonding between them and the matrix material.

[0028] In some preferred embodiments of the present invention, the device to be processed is preferably first broken into small pieces, and then placed in a nanobubble aqueous solution for treatment. This allows the nanobubbles to act more quickly and fully on the injection molded parts and / or glued parts in the device, thereby improving the effect of deplasticization and degumming. In the present invention, there is no limit to the size and shape of the broken pieces, for example, the device to be processed can be cut into small cubes of size <10cm*10cm.

[0029] In some embodiments of the present invention, when heating is performed during the soaking process, the heating temperature is preferably not less than 180°C. In some preferred embodiments of the present invention, the heating temperature can be 180°C to 800°C, such as 180°C to 700°C, such as 180°C to 600°C, such as 180°C to 500°C, such as 180°C to 400°C, such as 180°C to 300°C, such as about 180°C, about 200°C, about 220°C, about 240°C, about 250°C, about 280°C, etc., but are not limited to the listed values, and other unlisted values ​​or ranges within the numerical range are also applicable. The heating treatment helps to soften the injection molded parts and glued parts in the waste electronic equipment, making them more susceptible to external forces, thereby helping to improve the effects of deplasticization and degumming.

[0030] In some embodiments of the present invention, when heating is performed during the soaking process, the stirring speed is preferably not less than 100 rpm. In some preferred embodiments of the present invention, the stirring speed can be 100 rpm to 2000 rpm, such as 200 rpm to 2000 rpm, 300 rpm to 2000 rpm, 400 rpm to 2000 rpm, 500 rpm to 2000 rpm, 500 rpm to 1500 rpm, 500 rpm to 1000 rpm, 500 rpm to 800 rpm, such as about 500 rpm, about 550 rpm, about 600 rpm, about 650 rpm, about 700 rpm, about 750 rpm, about 800 rpm, etc., but is not limited to the listed values, and other unlisted values ​​or ranges within the numerical range are equally applicable.

[0031] In some embodiments of the present invention, the device to be treated is preferably immersed in the nanobubble solution for no less than 1 hour. In some preferred embodiments of the present invention, the immersion time may be from 1 hour to 8 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, etc., but is not limited to the listed values, and other values ​​or ranges not listed within the numerical range are also applicable.

[0032] In some embodiments of the present invention, after the immersion treatment is completed, the solution is filtered to obtain deplasticized and degummed waste components.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. Compared with the traditional method of applying volatile non-polar / polar solvents to recycle waste electronic equipment, the present invention uses nanobubble solution to recycle waste electronic equipment, which only requires water, energy and air, and does not require the use of volatile non-polar / polar solvents, which not only reduces pollution to the environment but also has good economic efficiency.

[0035] 2. Compared with traditional cleaning of waste electronic equipment, the cleaning method using nanobubble solution provided by the present invention can achieve plastic and glue removal of various types of injection molded parts, screen components, Apple Card, Airpods and other electronic products with only one step of cleaning, and the cleaning effect is better; in addition, batch processing can be carried out, which greatly shortens the process route of recycling waste electronic equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is the process route diagram of the present invention;

[0037] Figure 2 is the Zeta potential diagram of the nanobubble aqueous solution in Example 1;

[0038] Figure 3 is the particle size distribution diagram of nanobubbles in Example 1;

[0039] Figure 4 The electronic waste (a) before treatment and the electronic waste (b) after treatment in Example 1;

[0040] Figure 5 The electronic waste (a) before treatment and the electronic waste (b) after treatment in Comparative Example 1;

[0041] Figure 6 The electronic waste (a) before treatment and the electronic waste (b) after treatment in Comparative Example 2;

[0042] Figure 7 The electronic waste (a) before treatment and the electronic waste (b) after treatment in Example 2;

[0043] Figure 8 The electronic waste (a) before treatment and the electronic waste (b) after treatment in Comparative Example 3;

[0044] Fig. 9 The electronic waste (a) before treatment and the electronic waste (b) after treatment in Comparative Example 4;

[0045] Fig.10 The Zeta potential (a) of the nanobubble water before use and the Zeta potential (b) after use in Example 3;

[0046] Fig.11 The electronic waste (a) before treatment and the electronic waste (b) after treatment in Example 3. DETAILED DESCRIPTION

[0047] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0049] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0050] Example 1

[0051] This embodiment provides a method for efficiently separating injection molded parts / adhesive parts using a nanobubble aqueous solution, comprising the following steps:

[0052] S1. An anionic surfactant was added to deionized water at a volume ratio of 1:200, and high-speed shearing was performed at 10,000 rpm to obtain a nanobubble aqueous solution with an average Zeta potential of -35 mV and an average particle size of 106.2 nm.

[0053] S2. Place three types of waste electronic devices, namely, screen components with positive charges on the surface, Apple Card, and iPad metal back cover, into the nanobubble aqueous solution prepared in step S1, treat them at a temperature of 200° C. and a rotation speed of 500 rpm for three hours, and then filter.

[0054] Figure 2 and Figure 3 The zeta potential of the nanobubble aqueous solution and the particle size distribution of the nanobubbles prepared in Example 1 are shown respectively. As can be seen from the figure, in the nanobubble aqueous solution, the average particle size of the nanobubbles is 106.2 nm, and the average zeta potential of the nanobubble aqueous solution is -35 mV.

[0055] Figure 4 The state diagram of the waste electronic equipment before and after the treatment of Example 1 is shown. It can be seen from the figure that after being treated with the nanobubble aqueous solution, the three electronic devices with positive charges on the surface have achieved plastic removal and degumming, and achieved efficient separation of plastic and matrix materials.

[0056] Comparative Example 1

[0057] This comparative example provides a method for efficiently separating injection molded parts / adhesive parts using a nanobubble aqueous solution, comprising the following steps:

[0058] S1. A cationic surfactant was added to deionized water at a volume ratio of 1:200, and high-speed shearing was performed at 10,000 rpm to obtain a nanobubble aqueous solution with an average Zeta potential of +31 mV and an average particle size of 112 nm.

[0059] S2. Place three types of waste electronic devices, namely, screen components with positive charges on the surface, Apple Card, and iPad metal back cover, into the nanobubble aqueous solution prepared in step S1, treat them at a temperature of 200° C. and a rotation speed of 500 rpm for three hours, and then filter.

[0060] Figure 5 The state diagram of the waste electronic equipment before and after the treatment of Comparative Example 1 is shown. As can be seen from the figure, the nanobubble solution treatment has a poor deplasticization and degumming effect on the substrate material with positive charge on the surface.

[0061] The above results show that when the nanobubble solution and the waste electronic equipment carry the same electrical charge (positive charge), the nanobubble solution has a poor treatment effect on the waste electronic equipment due to the repulsion between like charges.

[0062] Comparative Example 2

[0063] This comparative example provides a method for efficiently separating injection molded parts / adhesive parts using a nanobubble aqueous solution, comprising the following steps:

[0064] S1. A cationic surfactant was added to deionized water at a volume ratio of 1:200, and high-speed shearing was performed at 500 rpm to obtain a nanobubble aqueous solution with an average Zeta potential of -15 mV and an average particle size of 329 nm.

[0065] S2. Place three types of waste electronic devices, namely, screen components with positive charges on the surface, Apple Card, and iPad metal back cover, into the nanobubble aqueous solution prepared in step S1, treat them at a temperature of 200° C. and a rotation speed of 500 rpm for three hours, and then filter.

[0066] Figure 6The state diagram of the waste electronic equipment before and after the treatment of Comparative Example 2 is shown. As can be seen from the figure, the nanobubble solution treatment has a poor effect on the deplasticization and degumming of the base material.

[0067] The above results show that when the absolute value of the zeta potential of the nanobubble solution is low (<25mV) and the average particle size is large (>200nm), the impact of the nanobubbles on the plastic parts and adhesive parts in the waste electronic equipment is small, which leads to poor treatment effect on the waste electronic equipment.

[0068] Example 2

[0069] This embodiment provides a method for efficiently separating injection molded parts / adhesive parts using a nanobubble aqueous solution, comprising the following steps:

[0070] S1. A cationic surfactant was added to deionized water at a volume ratio of 1:200, and high-speed shearing was performed at 10,000 rpm to obtain a nanobubble aqueous solution with an average Zeta potential of +31 mV and an average particle size of 112 nm.

[0071] S2. Place the waste electronic devices such as Airpods and charger plugs with negative charges on the surface into the nanobubble aqueous solution prepared in step S1, treat at a temperature of 200° C. and a rotation speed of 500 rpm for three hours, and then filter.

[0072] Figure 7 The state diagrams of two kinds of waste electronic equipment before and after treatment in Example 2 are shown. It can be seen from the figure that both kinds of waste electronic equipment with negative surface charge have achieved good plastic and glue removal.

[0073] Comparative Example 3

[0074] This comparative example provides a method for efficiently separating injection molded parts / adhesive parts using a nanobubble aqueous solution, comprising the following steps:

[0075] S1. A cationic surfactant was added to deionized water at a volume ratio of 1:200, and high-speed shearing was performed at 500 rpm to obtain a nanobubble aqueous solution with an average zeta potential of +15 mV and an average particle size of 329 nm.

[0076] S2. Place the waste electronic devices such as Airpods and charger plugs with negative charges on the surface into the nanobubble aqueous solution prepared in step S1, treat at a temperature of 200° C. and a rotation speed of 500 rpm for three hours, and then filter.

[0077] Figure 8 The state diagrams of two types of waste electronic equipment before and after treatment in Comparative Example 3 are shown. As can be seen from the figure, the nanobubble solution has a poor deplasticizing and degumming effect on the base material.

[0078] The above results show that when the absolute value of the zeta potential of the nanobubble solution is low (<25mV) and the average particle size is large (>200nm), the impact of the nanobubbles on the plastic parts and adhesive parts in the waste electronic equipment is small, which leads to poor treatment effect on the waste electronic equipment.

[0079] Comparative Example 4

[0080] This comparative example provides a method for efficiently separating injection molded parts / adhesive parts using a nanobubble aqueous solution, comprising the following steps:

[0081] S1. An anionic surfactant was added to deionized water at a volume ratio of 1:200, and high-speed shearing was performed at 10,000 rpm to obtain a nanobubble aqueous solution with an average zeta potential of -35 mV and an average particle size of 106.2 nm.

[0082] S2. Place the waste electronic devices such as Airpods and charger plugs with negative charges on the surface into the nanobubble aqueous solution prepared in step S1, treat at a temperature of 200° C. and a rotation speed of 500 rpm for three hours, and then filter.

[0083] Fig. 9 The state diagrams of two types of waste electronic equipment before and after treatment in Comparative Example 4 are shown. As can be seen from the figure, the nanobubble solution has a poor deplasticizing and degumming effect on the substrate material with negative charge on the surface.

[0084] The above results show that when the nanobubble solution and the waste electronic equipment carry the same electrical charge (negative charge), the nanobubble solution has a poor treatment effect on the waste electronic equipment due to the repulsion between like charges.

[0085] Example 3

[0086] In order to verify the cyclic stability of the nanobubble aqueous solution, the nanobubble solution after the first separation in Example 1 was filtered, and then the screen assembly, Apple Card, iPad metal back cover and other waste electronic devices with positive surface charges were treated again at a temperature of 200°C and a rotation speed of 500 rpm for three hours, and then filtered.

[0087] Fig.10 The zeta potential before and after the treatment of the nanobubble aqueous solution in Example 3 is shown. As can be seen from the figure, after the nanobubble solution has finished treating the waste electronic equipment, the absolute value of the zeta potential becomes larger.

[0088] Fig.11The state diagram of waste electronic equipment before and after treatment is shown. It can be seen from the figure that the nanobubble solution still has a good separation effect and good cycle stability after the waste electronic equipment is treated.

[0089] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. Application of nanobubble solution in separating injection molded parts / bonded parts.

2. Application of nanobubble solution in recycling of waste electronic equipment.

3. The use according to claim 1 or 2, It is characterized in that The absolute value of the Zeta potential of the nanobubble solution is not less than 25 mV; and in the nanobubble solution, the average particle size of the nanobubbles does not exceed 200 nm.

4. The use according to claim 1 or 2, It is characterized in that The nanobubble solution is an aqueous solution or an aqueous solution doped with nanobubbles; and / or, The gas in the nanobubbles includes at least one of air, nitrogen, oxygen, ozone, carbon dioxide, nitrogen dioxide, nitric oxide, and inert gas.

5. A method for separating injection molded parts / adhesive parts using nanobubble solution, It is characterized in that include: The device to be processed is placed in the nanobubble solution for immersion, and is heated and stirred during the immersion process; Wherein, the device to be treated and the nanobubble solution have charges of opposite electrical properties; The absolute value of the Zeta potential of the nanobubble solution is not less than 25 mV; and in the nanobubble solution, the average particle size of the nanobubbles does not exceed 200 nm.

6. A method for separating injection molded parts / adhesive parts using nano bubble solution according to claim 5, It is characterized in that The device comprises waste electronic equipment; and / or, Before the device is placed in the nanobubble solution, it is first broken into small pieces; the size of the small pieces does not exceed 10 cm*10 cm.

7. A method for separating injection molded parts / adhesive parts using nano bubble solution according to claim 5, It is characterized in that The nanobubble solution is an aqueous solution or an aqueous solution doped with nanobubbles; and / or, The gas in the nanobubbles includes at least one of air, nitrogen, oxygen, ozone, carbon dioxide, nitrogen dioxide, nitric oxide, and inert gas.

8. A method for separating injection molded parts / adhesive parts using nano bubble solution according to claim 5, It is characterized in that The heating temperature is 180°C to 800°C.

9. A method for separating injection molded parts / adhesive parts using nano bubble solution according to claim 5, It is characterized in that The soaking time is 1 to 8 hours.

10. A method for separating injection molded parts / adhesive parts using nano bubble solution according to claim 5, It is characterized in that After the soaking is completed, filtering is performed to obtain the deplasticized and degummed waste components.

Citation Information

Patent Citations

  • Photoresist removing device and method for removing photoresist

    CN111610698A

  • Method for leaching valuable metals from battery using nanobubbles

    CN113025825A

  • Novel ultrasonic coffee bean pectin separation device and separation method thereof

    CN115530279A

  • Method for separating positive electrode material and aluminum foil of waste lithium battery by using micro-nano bubbles

    CN116111225A

  • Method foe removing radioactive substance

    JP2016142599A