Copper / diamond composite material with nano gradient interface and preparation method of copper / diamond composite material
By constructing a nano-gradient interface through phonon mismatch model design and coating method, combined with the gas pressure impregnation method, the thermal conductivity of the diamond/copper composite material was improved, the problem of interface thermal resistance optimization was solved, and higher thermal conductivity was achieved and heat transfer efficiency.
Patent Information
- Application Number
- CN202410890244.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to further improve the thermal conductivity of diamond/copper composite materials with existing technology, mainly because the interface thermal resistance is difficult to optimize.
The phonon mismatch model is used to design the nano-gradient interface structure, and the carbide film is plated on the surface of the diamond particles through the coating method. The copper/diamond composite material with the nano-gradient interface is prepared by combining the gas pressure infiltration method to control the interface thermal conductivity and carbide. Layer thickness and proportions.
It significantly improves the thermal conductivity of copper/diamond composite materials, achieves higher interface thermal conductivity and faster heat transfer efficiency, and solves the problem of difficulty in improving thermal conductivity in traditional methods.
Smart Images

Figure CN118720105A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a copper / diamond composite material with a nano gradient interface and a preparation method thereof. Background Art
[0002] With the development of integration technology and microelectronic packaging technology, the "high performance and high integration" of semiconductor devices and chips have led to a continuous increase in power density. High thermal conductivity electronic packaging heat dissipation materials have become a guarantee for solving the efficient heat dissipation of devices and their reliability development. Electronic packaging heat dissipation materials have gone through multiple generations of development, such as Invar and Kovar alloys, Cu / W and Cu / Mo alloys, and Al / SiC and Cu / Si metal-based composite materials. The thermal conductivity is lower than 300 W / mK, which is difficult to meet the heat dissipation requirements of high-power devices. In recent years, composite materials prepared by combining high thermal conductivity (2000W / mK) and low thermal expansion coefficient (1.0ppm / K) diamond as a reinforcement with silver, copper and aluminum matrices have a thermal conductivity of 500-800W / mK. At the same time, the thermal expansion coefficient can be flexibly adjusted, which can be well matched with various levels of packaging materials. It has become an ideal packaging material for microwave solid-state power amplifiers in modern satellite communications, radars and electronic warfare fields.
[0003] At present, the traditional method of preparing diamond / copper composite materials has high interfacial thermal resistance and lacks the basis for interface design, which makes it difficult to further improve the thermal conductivity of the composite materials. For example, the Chinese invention patent with publication number CN105568037A proposes a method for preparing a diamond / copper composite material with higher thermal conductivity by chromium plating on the surface of diamond particles and modifying the interface by gas pressure infiltration. Although the interfacial thermal resistance is reduced by chromium plating modification, this method lacks theoretical data support in the early stage, so it is difficult to optimize the interfacial thermal resistance to the minimum, and it is difficult to further improve the thermal conductivity of the composite material. In view of the above shortcomings, the present invention proposes a copper / diamond composite material with a nano-gradient interface and a preparation method thereof through theoretical support. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention provides a copper / diamond composite material with a nano-gradient interface and a preparation method thereof, which solves the technical problem that it is difficult to further improve the thermal conductivity of the composite material in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a copper / diamond composite material with a nano-gradient interface, comprising the following steps: S1. Design nano-gradient interface structure and calculate interface thermal conductivity using phonon mismatch model; S2, according to the nano-gradient interface structure designed in step S1 and the calculation result of the interface thermal conductivity, a carbide film is sequentially plated on the surface of the diamond particles by a coating method to construct a nano-gradient interface structure; S3, preheating the furnace body; S4, filling the diamond particles with the nano-gradient interface structure in step S2 into a mold, placing the filled mold in a graphite sleeve, and then placing the entire filled mold in an induction heating zone of a high-pressure gas-assisted infiltration device; S5. Evacuate the furnace body. When the vacuum in the furnace reaches the conditions required for the experiment, heat the mold and keep it warm. Open the pressurized gas system to inject high-purity gas into the furnace for pressurization. When the gas in the furnace reaches a certain pressure, close the pressurized gas system and keep it warm and pressurized. After the heat preservation and pressure maintenance, cool the mold to room temperature, take it out and demould it to obtain a copper / diamond composite material with a nano-gradient interface.
[0006] Furthermore, the particle size of the diamond particles is 50-1000 μm.
[0007] Furthermore, in step S1, the thickness of the nano-gradient interface structure is less than 1000 nm, and the number of layers of the nano-gradient interface structure is greater than or equal to 2.
[0008] Furthermore, in step S2, the coating method is any one or more of molten salt low-temperature sintering, magnetron sputtering, physical vapor deposition, chemical vapor deposition, ion beam sputtering, atomic layer deposition, electron beam evaporation or ion-assisted deposition.
[0009] Further, in step S2, the carbide film is chromium carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, silicon carbide, boron carbide, titanium carbide or molybdenum carbide; The coating sequence of the carbide film on the surface of the diamond particles is from high thermal conductivity carbide to low thermal conductivity carbide or from low thermal conductivity carbide to high thermal conductivity carbide.
[0010] Furthermore, in step S3, the pre-charging temperature of the furnace body is 80-1100° C., and the preheating time is 1-120 min.
[0011] Furthermore, in step S5, the vacuum degree of the furnace body is evacuated to less than 10 Pa, and high-purity gas such as nitrogen or argon is injected into the furnace.
[0012] Furthermore, in step S5, the heating, pressurizing and heat preservation method is: starting from the preheating temperature, the temperature is increased to 1050-1200°C at a heating rate of 1-20°C / min, and the temperature is kept at this temperature for 0.1-4h; after the previous stage of heat preservation is completed, a pressure of 0.1-5MPa is immediately applied to the furnace and the pressure is maintained for 0.1-12h.
[0013] By means of the above technical solution, the present invention provides a copper / diamond composite material with a nano-gradient interface and a preparation method thereof, which has at least the following beneficial effects: 1. The present invention designs the nano-gradient interface structure and calculates the interface thermal conductivity of the copper / diamond composite material through the phonon mismatch model, effectively screening out the composite material with high interface thermal conductivity, and theoretically solves the problem that the interface thermal conductivity of the composite material is difficult to improve.
[0014] 2. The nano-stable gradient carbide interface constructed by the coating method between the diamond particles and the copper matrix of the present invention has the property of gradient heat transfer. Due to this unique heat transfer characteristic, compared with the traditional double interface structure, the thermal conductivity is higher and the heat transfer efficiency is faster, which can give full play to the high thermal conductivity of the diamond particles and greatly improve the thermal conductivity of the copper / diamond composite material.
[0015] 3. The present invention introduces a gas pressure infiltration method to fully combine the diamond particles with a nano-gradient carbide layer and the copper matrix. The degree of gradient interface diffusion reaction between the copper matrix and the diamond particles is controlled by the insulation time and the gas pressure, thereby obtaining a copper / diamond composite material with high interface bonding strength. The difficult problem of increasing the thermal conductivity of the composite material is solved by introducing a nano-thick carbide film at the interface. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings: Figure 1 A flow chart for preparing a copper / diamond composite material for the present invention; Figure 2 Schematic diagram of the formation process of a representative nano gradient interface structure of the present invention. DETAILED DESCRIPTION
[0017] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] This embodiment proposes a copper / diamond composite material with a nano-gradient interface, such as Figure 2As shown, the copper / diamond composite material comprises a nano-gradient interface structure constructed by sequentially coating carbide films on the surface of diamond particles, which includes: 50nm titanium carbide and 50-80nm chromium carbide layers are sequentially coated on the surface of diamond particles with a particle size of 20-900μm to form a copper / diamond composite material with a nano-gradient interface structure; or 100nm zirconium carbide and 40-100nm titanium carbide layers are sequentially coated on the surface of diamond particles with a particle size of 20-900μm to form a copper / diamond composite material with a nano-gradient interface structure; or 30nm titanium carbide, 50nm chromium carbide, and 50-80nm molybdenum carbide layers are sequentially coated on the surface of diamond particles with a particle size of 20-900μm to form a copper / diamond composite material with a nano-gradient interface structure.
[0019] The specific implementation methods for preparing the copper / diamond composite material are given through Examples 1 to 3. Figure 1 As shown, the preparation method uses a phonon mismatch model to design a nano-gradient interface structure and calculate the interface thermal conductivity. According to the calculation results, a gradient carbide film is plated on diamond particles by a coating method to form a nano-gradient interface structure. The diamond particles plated with the gradient carbide film are placed in a mold. After preheating the furnace body, a gas pressure infiltration method is used to compound the copper matrix and the diamond particles to obtain a copper / diamond composite material. The nano-gradient interface thermal conductivity of the composite material is regulated by adjusting the ratio and thickness of the carbide films and the gas pressure infiltration parameters, thereby obtaining a copper / diamond composite material with high thermal conductivity. Embodiment 1
[0020] The acoustic mismatch model (AMM) was used to calculate the interfacial thermal conductance of copper / diamond composite materials with four gradient interface structures, with 50nm titanium carbide and 50-80nm chromium carbide layers. According to the above calculation results, 50nm titanium carbide, 50nm or 60nm or 70nm or 80nm chromium carbide layers were coated on the surface of diamond particles with a particle size of 230μm, and the coated diamond particles were filled in the mold. Then the filled mold was placed in the graphite sleeve and the pure copper block was placed on the top of the mold. Then the filled mold was placed in the induction heating area of the high-pressure gas-assisted infiltration device, and the vacuum system and the pressurized gas system were connected. The vacuum system was turned on and the furnace body was evacuated until the vacuum degree was less than 10Pa. The circulating water was turned on, the induction heater was started, and the mold was heated to 700℃ and kept warm for 10min. The pressurized gas charging system was turned on to inject high-purity argon into the furnace body. When the gas pressure in the furnace reached 1.0 MPa, the pressurized gas charging system was turned off and the temperature and pressure were kept for 30 minutes. The heating was stopped. When the furnace temperature dropped below 100°C, the circulating water was turned off, the mold was removed and demolded to obtain a copper / diamond composite material product with a nano-gradient interface structure. The thermal conductivity of the prepared copper / diamond composite material was 668W / mK. Embodiment 2
[0021] The phonon mismatch model is used to calculate the interfacial thermal conductivities of four types of gradient interface structure copper / diamond composite materials with thicknesses of 100nm zirconium carbide and 40-100nm titanium carbide layers. According to the above calculation results, 100nm zirconium carbide, 40nm or 60nm or 80nm or 100nm titanium carbide layers are coated on the surface of diamond particles with a particle size of 180μm, and the coated diamond particles are filled in the mold. The filled mold is placed in a graphite sleeve and a pure copper block is placed on the upper part of the mold. The filled mold is then placed in the induction heating area of the high-pressure gas-assisted infiltration device, and the vacuum system and the pressurized gas system are connected. The vacuum system is turned on and the furnace body is evacuated until the vacuum degree is less than 10Pa. The circulating water is turned on, the induction heater is started, and the mold is heated to 700℃ and kept warm for 10min. The pressurized gas system is turned on to inject high-purity argon into the furnace body. When the gas pressure in the furnace reaches 1.0MPa, the pressurized gas system is turned off and the heat and pressure are maintained for 30min. Stop heating, and when the furnace temperature drops below 100°C, turn off the circulating water, take out the mold and demould, and obtain a copper / diamond composite material product with a nano-gradient interface structure. The thermal conductivity of the prepared copper / diamond composite material is 703W / mK. Embodiment 3
[0022] The phonon mismatch model is used to calculate the interfacial thermal conductance of four gradient interface structure copper / diamond composite materials with thicknesses of 30nm titanium carbide, 50nm chromium carbide, and 50-80nm molybdenum carbide layers. According to the above calculation results, 30nm titanium carbide, 50nm chromium carbide, 50nm or 60nm or 70nm or 80nm molybdenum carbide are plated on the surface of diamond particles with a particle size of 430μm, and the coated diamond particles are filled in the mold. The filled mold is placed in a graphite sleeve and a pure copper block is placed on the upper part of the mold. Then the entire filled mold is placed in the induction heating area of the high-pressure gas-assisted infiltration device, and the vacuum system and the pressurized gas system are connected. Turn on the vacuum system and evacuate the furnace until the vacuum degree is less than 10Pa. Turn on the circulating water, start the induction heater, and heat the mold to 800℃ for 10 minutes. The pressurized gas charging system was turned on to inject high-purity argon into the furnace body. When the gas pressure in the furnace reached 1.0 MPa, the pressurized gas charging system was turned off and the temperature and pressure were kept for 30 minutes. The heating was stopped. When the furnace temperature dropped below 100°C, the circulating water was turned off, the mold was removed and demolded, and a copper / diamond composite material product with a nano-gradient interface was obtained. The thermal conductivity of the prepared copper / diamond composite material was 732 W / mK. Comparative Example 1
[0023] The interfacial thermal conductivity of the copper / diamond composite material with a silicon carbide interface structure of 100 nm thickness was calculated using the phonon mismatch model. According to the above calculation results, a 100 nm silicon carbide layer was plated on the surface of diamond particles with a particle size of 230 μm, the coated diamond particles were filled in the mold, the filled mold was placed in a graphite sleeve and a pure copper block was placed on the upper part of the mold, and then the entire filled mold was placed in the induction heating area of the high-pressure gas-assisted infiltration device, and the vacuum system and the pressurized gas system were connected. The vacuum system was turned on and the furnace body was vacuumed until the vacuum degree was less than 10 Pa. The circulating water was turned on, the induction heater was started, and the mold was heated to 700 ° C and kept warm for 10 minutes. The pressurized gas system was turned on and high-purity argon was injected into the furnace body. When the gas pressure in the furnace reached 1.0 MPa, the pressurized gas system was turned off and kept warm and pressurized for 30 minutes. Stop heating, turn off the circulating water when the furnace temperature drops below 100 ° C, take out the mold and demold, and obtain a copper / diamond composite material product with a silicon carbide interface structure. The thermal conductivity of the prepared copper / diamond composite material is 442 W / mK. Comparative Example 2
[0024] The interfacial thermal conductivity of the copper / diamond composite material with a nickel carbide interface structure of 100nm thickness was calculated using the phonon mismatch model. According to the above calculation results, 100nm nickel carbide was plated on the surface of diamond particles with a particle size of 180μm, the coated diamond particles were filled in the mold, the filled mold was placed in a graphite sleeve and a pure copper block was placed on the upper part of the mold, and then the entire filled mold was placed in the induction heating area of the high-pressure gas-assisted infiltration device, and the vacuum system and the pressurized gas system were connected. The vacuum system was turned on and the furnace body was vacuumed until the vacuum degree was less than 10Pa. The circulating water was turned on, the induction heater was started, and the mold was heated to 700℃ and kept warm for 10min. The pressurized gas system was turned on and high-purity argon was injected into the furnace body. When the gas pressure in the furnace reached 1.0MPa, the pressurized gas system was turned off and kept warm and pressurized for 30min. Stop heating, turn off the circulating water when the furnace temperature drops below 100℃, take out the mold and demold, and obtain a copper / diamond composite material product with a nickel carbide interface structure. The thermal conductivity of the prepared copper / diamond composite material is 482 W / mK. Comparative Example 3
[0025] The interfacial thermal conductivity of the gradient interface structure copper / diamond composite material with a thickness of 100nm tungsten carbide was calculated using the phonon mismatch model. According to the above calculation results, 100nm tungsten carbide was plated on the surface of diamond particles with a particle size of 430μm, the coated diamond particles were filled in the mold, the filled mold was placed in a graphite sleeve and a pure copper block was placed on the upper part of the mold, and then the entire filled mold was placed in the induction heating area of the high-pressure gas-assisted infiltration device, and the vacuum system and the pressurized gas system were connected. The vacuum system was turned on and the furnace body was vacuumed until the vacuum degree was less than 10Pa. The circulating water was turned on, the induction heater was started, and the mold was heated to 800℃ and kept warm for 10min. The pressurized gas system was turned on and high-purity argon was injected into the furnace body. When the gas pressure in the furnace reached 1.0MPa, the pressurized gas system was turned off and kept warm and pressurized for 30min. Stop heating, turn off the circulating water when the furnace temperature drops below 100℃, take out the mold and demold, and obtain a copper / diamond composite material product with a tungsten carbide interface structure. The thermal conductivity of the prepared copper / diamond composite material is 589 W / mK. Thermal conductivity testing
[0026] Thermal conductivity is tested in accordance with GB / T 39862-2021: 1. Thermal diffusivity The test was carried out according to the method specified in GB / T 22588.
[0027] 2. Specific heat capacity measurement: 2.1 The sample size is required to be circular, with a diameter between 5mm and 8mm, a thickness between 0.1mm and 0.8mm, and a surface parallelism deviation of less than 0.5% of the thickness; 2.2 Test: Dry the sample to constant weight at 105℃-110℃; 2.3 Weigh the sample mass and standard mass to an accuracy of 0.01 mg; 2.4 Select two covered platinum crucibles of similar mass as sample pools; 2.5 Set the heating rate of the instrument, heat from temperature Ti to temperature Tf at a heating rate of 10℃ / min, measure each power and record; 2.6 Change the thickness of the sample to be tested and calculate the specific heat capacity of the sample; 2.7 Perform linear fitting on the obtained data, and the obtained fitting curve is the specific heat capacity of the sample; 2.8 Bulk density Test according to the method specified in GB / T 25995; 2.9 Thermal conductivity calculate.
[0028] The test results are shown in Table 1.
[0029] Table 1 Thermal conductivity test results Group Thermal conductivity / W / mK Embodiment 1 668W / mK Embodiment 2 703W / mK Embodiment 3 732W / mK Comparative Example 1 442W / mK Comparative Example 2 482 W / mK Comparative Example 3 589W / mK in conclusion: The copper / diamond composite material with a nano-gradient interface structure of the present invention exhibits higher thermal conductivity than the copper / diamond composite material with a titanium carbide / zirconium carbide / tungsten carbide interface structure. Therefore, the nano-stable gradient carbide interface constructed between the diamond particles and the copper matrix by the coating method of the present invention has the property of gradient heat transfer. Due to this unique heat transfer characteristic, compared with the traditional double interface structure, the thermal conductivity is higher and the heat transfer efficiency is faster, and the high thermal conductivity of the diamond particles can be more fully utilized, greatly improving the thermal conductivity of the copper / diamond composite material.
[0030] The present invention introduces a gas pressure infiltration method to fully combine diamond particles with a nano-gradient carbide layer and a copper matrix, controls the degree of gradient interface diffusion reaction between the copper matrix and the diamond particles by heat preservation time and gas pressure, obtains a copper / diamond composite material with high interface bonding strength, and solves the problem of difficulty in improving the thermal conductivity of the composite material by introducing a nano-thick carbide film at the interface.
[0031] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a copper / diamond composite material with a nano-gradient interface, characterized in that: The following steps are involved: S1. Design nano-gradient interface structure and calculate interface thermal conductivity using phonon mismatch model; S2, according to the nano-gradient interface structure designed in step S1 and the calculation result of the interface thermal conductivity, a carbide film is sequentially plated on the surface of the diamond particles by a coating method to construct a nano-gradient interface structure; S3, preheating the furnace body; S4, filling the diamond particles with the nano-gradient interface structure in step S2 into a mold, placing the filled mold in a graphite sleeve, and then placing the entire filled mold in an induction heating zone of a high-pressure gas-assisted infiltration device; S5. Evacuate the furnace body. When the vacuum in the furnace reaches the conditions required for the experiment, heat the mold and keep it warm. Open the pressurized gas system to inject high-purity gas into the furnace for pressurization. When the gas in the furnace reaches a certain pressure, close the pressurized gas system and keep it warm and pressurized. After the heat preservation and pressure maintenance, cool the mold to room temperature, take it out and demould it to obtain a copper / diamond composite material with a nano-gradient interface.
2. The preparation method according to claim 1, characterized in that: The particle sizes of the diamond particles are 50-1000 μm.
3. The preparation method according to claim 1, characterized in that: In the step S1, the thickness of the nano-gradient interface structure is less than 1000 nm, and the number of layers of the nano-gradient interface structure is greater than or equal to 2.
4. The preparation method according to claim 1, characterized in that: In step S2, the coating method is any one or more of molten salt low-temperature sintering, magnetron sputtering, physical vapor deposition, chemical vapor deposition, ion beam sputtering, atomic layer deposition, electron beam evaporation or ion-assisted deposition.
5. The preparation method according to claim 1, characterized in that: In the step S2, the carbide film is chromium carbide, tantalum carbide, vanadium carbide, zirconium carbide, tungsten carbide, silicon carbide, boron carbide, titanium carbide or molybdenum carbide; The coating sequence of the carbide film on the surface of the diamond particles is from high thermal conductivity carbide to low thermal conductivity carbide or from low thermal conductivity carbide to high thermal conductivity carbide.
6. The preparation method according to claim 1, characterized in that: In the step S3, the pre-charging temperature of the furnace body is 80-1100° C., and the pre-heating time is 1-120 min.
7. The preparation method according to claim 1, characterized in that: In the step S5, the furnace body is evacuated to a vacuum degree less than 10 Pa, and high-purity gas such as nitrogen or argon is injected into the furnace.
8. The preparation method according to claim 1, characterized in that: In step S5, the heating, pressurizing and heat preservation method is: starting from the preheating temperature, the temperature is increased to 1050-1200°C at a heating rate of 1-20°C / min, and the temperature is kept at this temperature for 0.1-4h; after the previous stage of heat preservation is completed, a pressure of 0.1-5MPa is immediately applied to the furnace and the pressure is maintained for 0.1-12h.
9. A copper / diamond composite material with a nano-gradient interface, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Cited By
High-performance low-cost diamond copper heat sink material product and preparation method and application thereof
CN120772532A
Diamond metal composite material and preparation method thereof
CN120843875A