Preparation method of tungsten-silicon alloy powder

Through three steps of step calcination and ball milling, the problem of insufficient particle size and composition uniformity of tungsten-silicon alloy powder was solved, the efficient preparation of tungsten-silicon alloy powder was achieved, the target performance requirements were met and the production cost was reduced.

CN118720131APending Publication Date: 2024-10-01KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410943369.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the field of powder metallurgy, how to effectively prepare tungsten-silicon alloy powder with uniform particle size to improve target performance and reduce raw material consumption. In the existing technology, the difference in melting points between Si and W causes the volatilization of silicon elements, causing waste and insufficient performance.

Method used

Using the method of three step calcination treatment and ball mill crushing treatment, the tungsten powder and silicon powder are mixed through a V-shaped mixer, and the primary, secondary, and third calcination and cooling are performed, and the primary and secondary ball milling is combined to control the tungsten-silicon alloy powder. Particle size distribution to ensure the integrity of the alloying reaction and particle size uniformity.

Benefits of technology

It achieves particle size uniformity and composition uniformity of tungsten-silicon alloy powder, meets target performance requirements, reduces raw material consumption and production costs, and has excellent industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720131A_ABST
    Figure CN118720131A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of tungsten-silicon alloy powder, which comprises the following steps: (1) mixing tungsten powder and silicon powder, and calcining to obtain tungsten-silicon alloy; (2) the tungsten-silicon alloy obtained in the step (1) is subjected to ball milling and crushing treatment, and tungsten-silicon alloy powder is obtained; the calcination treatment comprises primary calcination, secondary calcination, tertiary calcination and cooling treatment which are sequentially carried out. The tungsten-silicon alloy powder prepared by the preparation method of the tungsten-silicon alloy powder provided by the invention is uniform in granularity, and meets the use requirements of preparing a tungsten-silicon alloy target material; and the preparation method is simple in process and low in cost, and has excellent industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and relates to a tungsten-silicon alloy, and in particular to a method for preparing tungsten-silicon alloy powder. Background Art

[0002] The semiconductor industry is the core industry of the information age. With the development of the semiconductor industry, integrated circuits, as the main products of the semiconductor industry, are gradually becoming more multifunctional and refined. Sputtered thin films are one of the important components of semiconductor components and are generally obtained by sputtering targets. Tungsten silicon alloy target is a new type of alloy target. As a good conductor for vacuum sputtering, it can be used in the field of electronic gate materials and electronic thin films. Tungsten silicon thin films have the characteristics of high electrical conductivity, good thermal stability and excellent chemical corrosion resistance, and are widely used in the field of integrated circuits.

[0003] In order to make the tungsten silicon alloy target material play a good role in vacuum sputtering, it is generally required that the tungsten silicon target material has a high density, no internal defects, and the internal free silicon is small and evenly distributed. Therefore, it is necessary to improve the performance of the target material from the raw material.

[0004] Alloy powder is the main raw material for preparing target materials. In the field of powder metallurgy, the powder particle size seriously affects the various properties of powder metallurgy products. How to obtain alloy powder with uniform particle size has always been a difficult problem in the field of powder metallurgy. W and Si can react to obtain tungsten silicon alloy, but the melting points of Si and W are quite different. Preparation through smelting will cause a large amount of silicon to volatilize, resulting in a waste of raw materials. How to prepare tungsten silicon alloy more efficiently is also particularly important.

[0005] Using alloy powder to prepare corresponding alloy blocks can greatly improve the quality and performance of products and enhance the alloying degree of products. In addition, alloy powder can also reduce the difficulty of product preparation, reduce the consumption and waste of raw materials, and reduce production costs.

[0006] Therefore, it is necessary to provide a preparation method that can regulate the quality and performance of alloy powders. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing tungsten silicon alloy powder. The preparation method provided by the present invention has low cost and can effectively control the particle size of the alloy powder, thereby reducing the consumption and waste of raw materials and achieving the effect of reducing costs and increasing efficiency.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for preparing tungsten-silicon alloy powder, the preparation method comprising the following steps:

[0010] (1) mixing tungsten powder and silicon powder, and then calcining to obtain tungsten silicon alloy;

[0011] (2) ball milling the tungsten silicon alloy obtained in step (1) to obtain the tungsten silicon alloy powder;

[0012] The calcination process includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling process performed sequentially.

[0013] In the present invention, firstly, a reasonable staged calcination treatment process route is designed through the binary alloy phase diagram of tungsten and silicon to obtain a tungsten-silicon alloy with a good looseness, and then combined with ball milling crushing treatment, the uniform and controllable tungsten-silicon alloy powder is achieved, which can well meet the requirements of different products on powder particle size, thereby obtaining an alloy with excellent performance; and the preparation method provided by the present invention is low-cost and has excellent industrial application prospects.

[0014] As a preferred technical solution of the present invention, the mass ratio of tungsten powder to silicon powder in step (1) is 1:10 to 30, for example, it can be 1:10, 1:14, 1:18, 1:22, 1:26 or 1:30, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] As a preferred technical solution of the present invention, the mixing in step (1) is carried out using a V-type powder mixer.

[0016] Preferably, the mixing time in step (1) is 12 to 24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] The present invention achieves complete mixing of tungsten powder and silicon powder by a V-shaped powder mixer, but the mixing time should not be too long to avoid agglomeration of silicon powder.

[0018] As a preferred technical solution of the present invention, the particle size range of the tungsten powder in step (1) is ≤80 μm, for example, it can be 80 μm, 70 μm, 60 μm, 50 μm, 40 μm, 30 μm or 20 μm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; preferably 50 to 60 μm.

[0019] Preferably, the particle size range of the silicon powder in step (1) is ≤100 μm, for example, it can be 100 μm, 90 μm, 80 μm, 70 μm, 60 μm, 50 μm, 40 μm, 30 μm or 20 μm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; preferably, it is 60 to 80 μm.

[0020] As a preferred technical solution of the present invention, the calcination treatment in step (1) is carried out in an oxygen-free environment.

[0021] Preferably, the oxygen-free environment includes a nitrogen gas environment and / or an inert gas environment.

[0022] As a preferred technical solution of the present invention, the heating rate of the primary calcination is 8 to 10°C / min, for example, it can be 8°C / min, 8.4°C / min, 8.8°C / min, 9.2°C / min, 9.6°C / min or 10°C / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0023] Preferably, the calcination temperature of the primary calcination is 900-1100°C, for example, 900°C, 950°C, 1000°C, 1050°C or 1100°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] Preferably, the holding time of the primary calcination is 50 to 70 min, for example, 50 min, 54 min, 58 min, 62 min, 66 min or 70 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] In the present invention, the primary calcination acts as a buffer step from low temperature to high temperature, allowing the equipment to enter the high temperature stage evenly; if the calcination temperature of the primary calcination is too high, it will cause the atoms to diffuse prematurely and produce partial alloying, and if the calcination temperature is too low, the buffer effect cannot be achieved; if the heating rate of the primary calcination is too high, it will cause a temperature charging process inside the calcination furnace, and if it is too low, it will extend the calcination time and cause waste.

[0026] Preferably, the heating rate of the secondary calcination is 3 to 5°C / min, for example, 3°C / min, 3.4°C / min, 3.8°C / min, 4.2°C / min, 4.6°C / min or 5°C / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] Preferably, the calcination temperature of the secondary calcination is 1200-1280°C, for example, 1200°C, 1220°C, 1240°C, 1260°C or 1280°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the holding time of the secondary calcination is 20 to 40 min, for example, 20 min, 24 min, 28 min, 32 min, 36 min or 40 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] In the present invention, the function of the secondary calcination is to provide activation energy for the diffusion of materials.

[0030] Preferably, the heating rate of the three calcinations is 3 to 5°C / min, for example, 3°C / min, 3.4°C / min, 3.8°C / min, 4.2°C / min, 4.6°C / min or 5°C / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] Preferably, the calcination temperature of the three calcinations is 1320-1380°C, for example, 1320°C, 1340°C, 1360°C or 1380°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the holding time for the three calcinations is 5.5 to 6.5 h, for example, 5.5 h, 5.7 h, 5.9 h, 6.1 h, 6.3 h or 6.5 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] In the present invention, the functions of the three calcinations are to cause alloying reaction between W and Si to produce WSi2 phase. If the heating rate in the three calcinations is too high, a large loss of Si will be caused, while if the heating rate is too low, the alloying rate of W and Si will be slow. If the calcination temperature of the three calcinations is too high, the calcination time will be increased and Si will evaporate in large quantities, while if the calcination temperature is too low, the alloying will not be complete.

[0034] Preferably, the terminal temperature of the cooling treatment is 350-400°C, for example, 350°C, 360°C, 370°C, 380°C, 390°C or 400°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] The calcination treatment of the present invention is carried out in a high-temperature muffle furnace, and a tungsten silicon alloy with a good looseness is prepared by three consecutive step-wise calcination treatments.

[0036] As a preferred technical solution of the present invention, the ball milling process in step (2) includes primary ball milling and secondary ball milling performed sequentially.

[0037] The present invention achieves the crushing and grinding of the tungsten silicon alloy obtained in step (1) by ball milling and crushing treatment to obtain alloy powder, thereby achieving uniform and controllable particle size of the alloy powder.

[0038] As a preferred technical solution of the present invention, the rotation speed of the primary ball mill is 150-160r / min, for example, it can be 150r / min, 152r / min, 154r / min, 156r / min, 158r / min or 160r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] Preferably, the time of the first ball milling is 50 to 70 min, for example, 501 min, 54 min, 58 min, 62 min, 66 min or 70 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0040] The present invention achieves the crushing of tungsten silicon alloy through high-speed primary ball milling. If the rotation speed is too high, the capacity in the ball mill jar will be high, and the powder will become compacted and sink to the bottom. If the rotation speed is too low, the particles will not be completely crushed.

[0041] Preferably, the rotation speed of the secondary ball milling is 100-120 r / min, for example, it can be 100 r / min, 104 r / min, 108 r / min, 112 r / min, 116 r / min or 120 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] Preferably, the secondary ball milling time is 2 to 3 hours, for example, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours or 3 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0043] The present invention achieves uniform and controllable alloy powder particle size through low-speed secondary ball milling. If the rotation speed is too high, it will lead to greater energy and further reduction of powder particle size. If the powder particle size is too small, it will cause powder agglomeration and sinking to the bottom during the crushing process, increasing the difficulty of powder extraction and the risk of powder scrapping. If the rotation speed is too low, the powder crushing uniformity cannot be improved and the particle size distribution is more dispersed.

[0044] As a preferred technical solution of the present invention, the mass ratio of the grinding balls used in the ball milling process in step (2) to the tungsten silicon alloy in step (1) is 3 to 5:1, for example, it can be 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1, 4.4:1, 4.6:1, 4.8:1 or 5:1, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 4:1.

[0045] The ball-to-material ratio in the ball mill crushing process of the present invention is 3 to 5:1. If the amount of grinding balls used is too low, the crushing effect cannot be achieved. If the quality of the grinding balls is too high, the degree of wear of the grinding balls will increase, the impurity content will increase, and the weight of the tank will be greatly increased, making the operation of the ball mill more difficult.

[0046] Preferably, the grinding balls used in the ball milling process in step (2) include zirconium oxide balls.

[0047] As a preferred technical solution of the present invention, the method for preparing tungsten silicon alloy powder provided by the present invention comprises the following steps:

[0048] (1) mixing tungsten powder with a particle size of ≤80 μm and silicon powder with a particle size of ≤100 μm in a V-type powder mixer at a mass ratio of 1:10 to 30 for 12 to 24 hours, and then calcining in an oxygen-free environment to obtain a tungsten-silicon alloy;

[0049] The calcination treatment includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling treatment performed in sequence; the heating rate of the primary calcination is 8-10°C / min, the calcination temperature is 900-1100°C, and the holding time is 50-70min; the heating rate of the secondary calcination is 3-5°C / min, the calcination temperature is 1200-1280°C, and the holding time is 20-40min; the heating rate of the tertiary calcination is 3-5°C / min, the calcination temperature is 1320-1380°C, and the holding time is 5.5-6.5h;

[0050] (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 3 to 5:1 and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder;

[0051] The rotation speed of the first ball milling is 150-160 r / min, and the time is 50-70 min; the rotation speed of the second ball milling is 100-120 r / min, and the time is 2-3 h.

[0052] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The particle size of the tungsten-silicon alloy powder obtained by the preparation method provided by the present invention is uniform, meeting the requirements for preparing tungsten-silicon alloy targets;

[0055] (2) The preparation method provided by the present invention has a simple process, low cost and excellent industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 is a microscopic enlarged image of the tungsten silicon alloy powder provided in Example 1 of the present invention;

[0057] Figure 2 This is a microscopic enlarged image of the tungsten silicon alloy provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0058] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0059] Example 1

[0060] This embodiment provides a method for preparing tungsten-silicon alloy powder, the preparation method comprising the following steps:

[0061] (1) mixing tungsten powder with a particle size of 80 μm and silicon powder with a particle size of 100 μm in a V-type powder mixer at a mass ratio of 1:20 for 18 hours, and then calcining in an oxygen-free environment to obtain a tungsten-silicon alloy;

[0062] The calcination treatment includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling treatment performed in sequence; the heating rate of the primary calcination is 10°C / min, the calcination temperature is 1000°C, and the holding time is 60min; the heating rate of the secondary calcination is 5°C / min, the calcination temperature is 1250°C, and the holding time is 30min; the heating rate of the tertiary calcination is 5°C / min, the calcination temperature is 1350°C, and the holding time is 6h;

[0063] (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 4:1 and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder;

[0064] The rotation speed of the first ball milling is 150 r / min, and the time is 60 min; the rotation speed of the second ball milling is 110 r / min, and the time is 2 h.

[0065] The microscopic enlarged image of the tungsten silicon alloy powder obtained in this embodiment is as follows: Figure 1 As shown in the figure, the microscopic enlarged image of the tungsten silicon alloy without ball milling is as follows Figure 2 shown.

[0066] Example 2

[0067] This embodiment provides a method for preparing tungsten-silicon alloy powder, the preparation method comprising the following steps:

[0068] (1) mixing tungsten powder with a particle size of 60 μm and silicon powder with a particle size of 80 μm in a V-type powder mixer at a mass ratio of 1:10 for 12 hours, and then calcining in an oxygen-free environment to obtain a tungsten-silicon alloy;

[0069] The calcination treatment includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling treatment performed in sequence; the heating rate of the primary calcination is 8°C / min, the calcination temperature is 900°C, and the holding time is 70min; the heating rate of the secondary calcination is 3°C / min, the calcination temperature is 1200°C, and the holding time is 40min; the heating rate of the tertiary calcination is 3°C / min, the calcination temperature is 1320°C, and the holding time is 6.5h;

[0070] (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 3:1 and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder;

[0071] The rotation speed of the first ball milling is 160 r / min, and the time is 50 min; the rotation speed of the second ball milling is 120 r / min, and the time is 2.5 h.

[0072] Example 3

[0073] This embodiment provides a method for preparing tungsten-silicon alloy powder, the preparation method comprising the following steps:

[0074] (1) mixing tungsten powder with a particle size of 50 μm and silicon powder with a particle size of 80 μm in a V-type powder mixer at a mass ratio of 1:30 for 24 hours, and then calcining in an oxygen-free environment to obtain a tungsten-silicon alloy;

[0075] The calcination treatment includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling treatment performed in sequence; the heating rate of the primary calcination is 9°C / min, the calcination temperature is 1100°C, and the holding time is 50min; the heating rate of the secondary calcination is 4°C / min, the calcination temperature is 1280°C, and the holding time is 20min; the heating rate of the tertiary calcination is 4°C / min, the calcination temperature is 1380°C, and the holding time is 5.5h;

[0076] (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 5:1 and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder;

[0077] The rotation speed of the first ball milling is 150 r / min, and the time is 70 min; the rotation speed of the second ball milling is 100 r / min, and the time is 3 h.

[0078] Example 4

[0079] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0080] In this embodiment, the particle size of the tungsten powder in step (1) is adjusted to 100 μm, and the particle size of the silicon powder is adjusted to 10 μm.

[0081] Example 5

[0082] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0083] In this embodiment, the particle size of the tungsten powder in step (1) is adjusted to 10 μm, and the particle size of the silicon powder is adjusted to 120 μm.

[0084] Example 6

[0085] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0086] In this embodiment, the heating rate of the primary calcination in step (1) is adjusted to 5°C / min.

[0087] Example 7

[0088] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0089] In this embodiment, the calcination temperature of the three calcinations in step (1) is adjusted to 1300°C.

[0090] Example 8

[0091] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0092] In this embodiment, the calcination temperature of the three calcinations in step (1) is adjusted to 1400°C.

[0093] Example 9

[0094] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0095] In this embodiment, the mass ratio of the grinding balls used in the ball milling process in step (2) to the tungsten silicon alloy in step (1) is adjusted to 2:1.

[0096] Example 10

[0097] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0098] In this embodiment, the mass ratio of the grinding balls used in the ball milling process in step (2) to the tungsten silicon alloy in step (1) is adjusted to 6:1.

[0099] Embodiment 11

[0100] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0101] In this embodiment, the rotation speed of the first ball milling in step (2) is adjusted to 140 r / min.

[0102] Example 12

[0103] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0104] In this embodiment, the rotation speed of the ball milling process in step (2) is adjusted to 150 r / min and the time is 3 h.

[0105] Example 13

[0106] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0107] In this embodiment, the rotation speed of the ball milling process in step (2) is adjusted to 110 r / min and the time is 3 h.

[0108] Comparative Example 1

[0109] This comparative example provides a method for preparing tungsten silicon alloy powder, which differs from Example 1 only in that:

[0110] In this comparative example, the calcination treatment in step (1) was adjusted as follows: heating to 1350° C. at a heating rate of 10° C. / min and maintaining the temperature for 7.5 h.

[0111] Comparative Example 2

[0112] This comparative example provides a method for preparing tungsten silicon alloy powder, which differs from Example 1 only in that:

[0113] In this comparative example, the calcination treatment in step (1) was adjusted as follows: heating to 1350° C. at a heating rate of 5° C. / min and keeping the temperature for 7.5 h.

[0114] Comparative Example 3

[0115] This comparative example provides a method for preparing tungsten silicon alloy powder, which differs from Example 1 only in that:

[0116] In this comparative example, the calcination treatment in step (1) is adjusted as follows: the calcination treatment is carried out at a vacuum degree of 10 Pa and a temperature of 1150° C. for 1.6 h, and the heating rate of the calcination treatment is 17° C. / min.

[0117] The test results of the tungsten-silicon alloy powder obtained by the preparation methods provided in the above embodiments and comparative examples are shown in Table 1.

[0118] Table 1

[0119] Powder particle size / μm Particle size distribution uniformity Composition uniformity Example 1 ≤18 More uniform More uniform Example 2 ≤25 More uniform More uniform Example 3 ≤12 More uniform More uniform Example 4 ≤18 More uniform Uneven Example 5 ≤18 More uniform Uneven Example 6 ≤25 More uniform Uneven Example 7 ≤20 More uniform Uneven Example 8 ≤35 Uneven Uneven Example 9 ≤30 Uneven Uneven Example 10 ≤7 Uneven Uneven Embodiment 11 ≤40 Uneven More uniform Example 12 10~40 Uneven More uniform Embodiment 13 10~30 Uneven More uniform Comparative Example 1 ≤23 More uniform Uneven Comparative Example 2 ≤30 Uneven Uneven Comparative Example 3 ≤30 Uneven Uneven

[0120] According to Table 1, we can know the following points:

[0121] (1) Comprehensive analysis of Examples 1-3 shows that the particle size distribution and composition distribution of the tungsten silicon alloy powder obtained by the preparation method provided by the present invention are uniform, the performance is good, and the use requirements for preparing tungsten silicon alloy targets are met;

[0122] (2) Comprehensive analysis of Example 1 and Examples 6-8 shows that the heating rate during the calcination process will affect the change of the reaction components. If the heating rate during a calcination process is too low, the reaction will be slow and the alloy will not be calcined thoroughly.

[0123] In addition, the highest temperature of the calcination treatment is the tertiary calcination temperature. If the tertiary calcination temperature is too high, the calcined alloy block will become hardened, increasing the uniformity of the subsequent crushing particle size. If the tertiary calcination temperature is too low, the reaction will not be complete and the composition will change.

[0124] Comprehensive analysis of Example 1 and Comparative Examples 1-3 shows that using a single heating rate to heat up to the calcination temperature three times will make the particle size distribution and composition distribution of the tungsten silicon alloy powder uneven;

[0125] This shows that the continuous step-type calcination treatment provided by the present invention is one of the important factors for controlling the particle size distribution and uniform composition distribution of the tungsten silicon alloy powder;

[0126] (3) Comprehensive analysis of Example 1 and Examples 9-13 shows that a too high or too low mass ratio of grinding balls to tungsten silicon alloy in the ball milling process will make the particle size distribution and component distribution of the tungsten silicon alloy powder uneven, and even affect the particle size range of the alloy powder;

[0127] As described in Example 11, when the speed of the primary ball milling is too high, the energy in the high-energy ball milling stage will be too high, resulting in uneven powder particle size and serious compaction of the powder in the ball milling jar.

[0128] As described in Examples 11-12, when a single ball milling speed is used to grind the tungsten silicon alloy, the separation particle size distribution range after ball milling is large, and there are many large particles, and it is impossible to obtain an alloy powder with a uniform particle size.

[0129] This shows that combining high-speed ball milling and low-speed ball milling for grinding is one of the important factors in controlling the particle size distribution and uniform composition distribution of tungsten silicon alloy powder.

[0130] In summary, the tungsten-silicon alloy powder preparation method provided by the present invention has uniform particle size, which meets the requirements for preparing tungsten-silicon alloy targets; and the preparation method has a simple process, low cost, and excellent industrial application prospects.

[0131] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing tungsten silicon alloy powder, characterized in that: The preparation method comprises the following steps: (1) mixing tungsten powder and silicon powder, and then calcining to obtain tungsten silicon alloy; (2) ball milling the tungsten silicon alloy obtained in step (1) to obtain the tungsten silicon alloy powder; The calcination process includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling process performed sequentially.

2. The preparation method according to claim 1, characterized in that: The mass ratio of the tungsten powder to the silicon powder in step (1) is 1:10 to 30.

3. The preparation method according to claim 1 or 2, characterized in that: The mixing in step (1) is carried out using a V-shaped powder mixer; Preferably, the mixing time in step (1) is 12 to 24 hours.

4. The preparation method according to any one of claims 1 to 3, characterized in that The particle size of the tungsten powder in step (1) is ≤80 μm, preferably 50 to 60 μm; Preferably, the particle size of the silicon powder in step (1) is ≤100 μm, preferably 60 to 80 μm.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The calcination treatment in step (1) is carried out in an oxygen-free environment; Preferably, the oxygen-free environment includes a nitrogen gas environment and / or an inert gas environment.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The heating rate of the primary calcination is 8 to 10°C / min; Preferably, the calcination temperature of the primary calcination is 900-1100°C; Preferably, the holding time of the primary calcination is 50 to 70 minutes; Preferably, the heating rate of the secondary calcination is 3-5°C / min; Preferably, the calcination temperature of the secondary calcination is 1200-1280°C; Preferably, the holding time of the secondary calcination is 20 to 40 minutes; Preferably, the heating rate of the three calcinations is 3-5°C / min; Preferably, the calcination temperature of the three calcinations is 1320-1380°C; Preferably, the holding time for the three calcinations is 5.5 to 6.5 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The ball milling process in step (2) includes primary ball milling and secondary ball milling performed sequentially.

8. The preparation method according to claim 7, characterized in that: The rotation speed of the first ball mill is 150-160 r / min; Preferably, the time of the first ball milling is 50 to 70 minutes; Preferably, the rotation speed of the secondary ball milling is 100-120 r / min; Preferably, the secondary ball milling time is 2 to 3 hours.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The mass ratio of the grinding balls used in the ball milling process of step (2) to the tungsten silicon alloy of step (1) is 3 to 5:1; Preferably, the grinding balls used in the ball milling process in step (2) include zirconia balls.

10. The preparation method according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: (1) mixing tungsten powder with a particle size of ≤80 μm and silicon powder with a particle size of ≤100 μm in a V-type powder mixer at a mass ratio of 1:10 to 30 for 12 to 24 hours, and then calcining in an oxygen-free environment to obtain a tungsten-silicon alloy; The calcination treatment includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling treatment performed in sequence; the heating rate of the primary calcination is 8-10°C / min, the calcination temperature is 900-1100°C, and the holding time is 50-70min; the heating rate of the secondary calcination is 3-5°C / min, the calcination temperature is 1200-1280°C, and the holding time is 20-40min; the heating rate of the tertiary calcination is 3-5°C / min, the calcination temperature is 1320-1380°C, and the holding time is 5.5-6.5h; (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 3 to 5:1, and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder; The rotation speed of the first ball milling is 150-160 r / min, and the time is 50-70 min; the rotation speed of the second ball milling is 100-120 r / min, and the time is 2-3 h.

Citation Information

Cited By

  • Cobalt-iron-boron target material and preparation method and application thereof

    CN119260002A

  • A cobalt iron boron target material, a preparation method thereof and application thereof

    CN119260002B