Graphene / Al2O3 / Cu composite material and preparation method
Through co-precipitation method and high-temperature catalytic technology, graphene and Al2O3 are evenly dispersed in copper powder, which solves the problem of uneven dispersion of graphene in dispersed copper, significantly improves the electrical and thermal conductivity of the composite material, and avoids the impact of graphene on the copper powder. modification treatment.
Patent Information
- Application Number
- CN202410766510.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the dispersion of graphene in solution is highly demanding and difficult to control, resulting in uneven dispersion in dispersed copper, affecting the electrical and thermal conductivity properties, and graphene needs to be modified to solve the problem of uniform dispersion. But this will sacrifice some conductive properties.
Al2O3/Cu/carbon source mixed powder is prepared by co-precipitation method, and graphene is grown in situ on the copper powder surface through high-temperature catalysis, combined with hot-pressing sintering to achieve uniform dispersion of graphene and Al2O3 and avoid modification of graphene. deal with.
The comprehensive performance of the composite material is significantly improved, with the tensile strength reaching more than 400MPa and the electrical conductivity reaching more than 90% IACS, while retaining the high electrical and thermal conductivity of graphene.
Smart Images

Figure BDA0004892675940000101
Abstract
Description
Technical Field
[0001] The present invention relates to the field of dispersion-strengthened copper, and in particular to a graphene / Al2O3 / Cu composite material and a preparation method thereof. Background Art
[0002] Dispersion-strengthened copper is a composite material that strengthens the copper matrix by introducing uniformly distributed, fine, and thermally stable reinforcement phase particles into the matrix. This type of material has high strength, high electrical conductivity, high thermal conductivity, and high softening temperature, and is widely used in the mechanical industry, electronics, and aerospace fields. The reinforcement particles in dispersion-strengthened copper greatly reduce its electrical and thermal conductivity, and cannot meet the requirements of high-strength and high-conductivity copper alloys.
[0003] Graphene is a two-dimensional nanomaterial composed of a single layer of carbon atoms. It has a fracture strength of 125GPa and a Young's modulus of about 1100GPa. It has excellent thermal conductivity and charge transport properties. It is an ideal new reinforcement for preparing high-strength and high-conductivity copper-based composite materials. Introducing graphene into dispersion-strengthened copper can improve its electrical and thermal conductivity and achieve high strength and high conductivity.
[0004] Dispersed copper is generally prepared by mechanical mixing or internal oxidation-reduction methods, but the mechanical mixing method often leads to agglomeration and uneven dispersion of dispersed phase alumina, resulting in a decrease in material performance. The internal oxidation-reduction method can achieve uniform dispersion of alumina, but in the internal oxidation process, if it is not properly controlled, it is easy to cause the alumina particles to grow, thereby affecting its dispersion strengthening effect.
[0005] The co-precipitation method for preparing dispersed copper can achieve uniform dispersion of alumina in copper, and the size and distribution state of alumina can also be well controlled. Therefore, it is an ideal method for preparing dispersion-strengthened copper alloys and a commonly used method for preparing graphene / Al2O3 / Cu composites.
[0006] The patent application number CN201710968906.6 in the prior art discloses a method for preparing graphene-enhanced ODS copper, wherein a composite powder of aluminum hydroxide, copper hydroxide and graphene is prepared by coprecipitation, and graphene-enhanced dispersed copper is obtained by reduction, molding, sintering and hot extrusion. This method can make graphene uniformly dispersed in the dispersed copper matrix, but it has high requirements on the dispersibility of graphene in the solution, and it is necessary to modify the graphene to a certain extent, which will sacrifice some of the conductive properties. In addition, the dispersion state and dispersion amount of graphene in the solution are difficult to control, which makes it difficult to accurately control the dispersion uniformity and introduction amount in the dispersed copper, which is not conducive to batch preparation.
[0007] In summary, the prior art needs to modify graphene to solve the problem of uniform dispersion of graphene in the solution, resulting in reduced electrical and thermal conductivity. At the same time, it is also unable to perfectly solve the problem of uniform dispersion in the solution, resulting in uneven dispersion of graphene in the copper matrix, and even problems such as agglomeration and curling.
[0008] In view of this, the present invention is proposed. Summary of the invention
[0009] The purpose of the present invention is to provide a graphene / Al2O3 / Cu composite material and a preparation method thereof, so as to solve the problem in the prior art that graphene needs to be modified to solve the uniform dispersion of graphene in a solution, resulting in reduced electrical and thermal conductivity, and also unable to perfectly solve the problem of uniform dispersion in the solution, resulting in uneven dispersion of graphene in a copper matrix, and even problems such as agglomeration and curling.
[0010] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0011] A method for preparing a graphene / Al2O3 / Cu composite material, the preparation method comprising the following steps:
[0012] S1. Co-precipitation: copper sulfate Cu(NO3)2 and ammonium aluminum sulfate NH4Al(SO4)2·12H2O are used to prepare a reaction mother liquor, ammonium bicarbonate NH4HCO3 is used to prepare a precipitant, polyvinyl alcohol and sucrose are added to the reaction mother liquor, and the precipitant is added after stirring evenly. After the addition is completed, the reaction is continued for 2 hours to obtain a mixed solution; the mixed solution is spray-granulated to obtain a granulated powder; the granulated powder is placed in a reduction furnace, first calcined, and then reduced to obtain an Al2O3 / Cu / carbon source mixed powder;
[0013] S2, high temperature catalysis: put the Al2O3 / Cu / carbon source mixed powder into a tube furnace, evacuate, then introduce argon and hydrogen, heat to 800°C, keep warm for 1 to 100 minutes, and then quickly cool to room temperature to obtain graphene / Al2O3 / Cu composite powder;
[0014] S3. Densification: hot pressing and sintering the graphene / Al2O3 / Cu composite powder to obtain a graphene / Al2O3 / Cu composite material.
[0015] The preparation method of the graphene / Al2O3 / Cu composite material of the present invention comprises steps S1 to S3 which are interrelated. In step S1, a coprecipitation method is used to prepare an Al2O3 / Cu / carbon source mixed powder to ensure uniform dispersion of Al2O3 in Cu. Meanwhile, sucrose, a soluble carbon source, is introduced during the coprecipitation process to uniformly disperse the carbon source in the Cu matrix. Then, in step S2, high temperature catalysis is performed to in-situ grow graphene on the surface of the copper powder to achieve uniform dispersion of the graphene. The graphene is prepared by an in-situ autogenous method without Graphene needs to be modified, so that the high electrical conductivity and high thermal conductivity of graphene are retained to the greatest extent; finally, the graphene / Al2O3 / Cu composite powder is hot-pressed and sintered by S3 to obtain a graphene / Al2O3 / Cu composite material; using the method of the present invention, first, graphene and Al2O3 can be evenly dispersed in the copper matrix, second, the comprehensive performance of the composite material can be significantly improved, and the tensile strength can reach more than 400MPa; third, it has high electrical conductivity, and the conductivity can reach more than 90%IACS.
[0016] Furthermore, in step S1, before adding polyvinyl alcohol and sucrose to the reaction mother liquor, the temperature of the mother liquor is controlled at 10-90°C.
[0017] Furthermore, in step S1, a precipitant is added to the reaction mother solution at a rate of 5 to 1000 ml / min. When the pH value of the final reaction solution reaches 7 to 10, the addition of the precipitant can be stopped.
[0018] Furthermore, in step S1, the spray granulation process is as follows: inlet air temperature is 100-300°C, outlet air temperature is 60-200°C, and atomizer frequency is 20-50 Hz.
[0019] Furthermore, in step S1, calcination is carried out under an argon atmosphere, and the calcination process is: firstly heating to 250°C and keeping the temperature for 4 hours to fully decompose the ammonium nitrate; then heating to 400-500°C and keeping the temperature for 1-6 hours.
[0020] Furthermore, in step S1, the reduction is carried out in a hydrogen atmosphere, and the reduction process is as follows: the temperature is 400-500° C., and the insulation time is 1-6 hours.
[0021] Furthermore, in step S2, the flow rate of argon gas is 10-500 ml / min, and the flow rate of hydrogen gas is 10-500 ml / min.
[0022] Furthermore, in step S3, the hot pressing sintering process is: pressure 30-50 MPa, temperature 750-950° C., and heat preservation time 1-10 hours.
[0023] Furthermore, in step S1, ammonium bicarbonate NH4HCO3 is used to prepare a precipitant, and the pH value is adjusted to 7-12 with aqueous ammonia.
[0024] In a second aspect of the present invention, a graphene / Al2O3 / Cu composite material is provided, wherein the graphene / Al2O3 / Cu composite material is prepared using any one of the methods for preparing the graphene / Al2O3 / Cu composite material.
[0025] The present invention proposes a graphene / Al2O3 / Cu composite material and a preparation method thereof. Compared with the prior art, the graphene / Al2O3 / Cu composite material and the preparation method thereof described in the present invention have the following beneficial effects:
[0026] (1) The graphene / Al2O3 / Cu composite material and preparation method described in the present invention improve the dispersion uniformity of the reinforcement phase: the present invention prepares Al2O3 / Cu / carbon source mixed powder by coprecipitation method to ensure the uniform dispersion of Al2O3 in Cu. At the same time, sucrose, a soluble carbon source, is introduced into the coprecipitation process to make it uniformly dispersed in the Cu matrix, and then graphene is grown in situ on the surface of the copper powder through high-temperature catalysis to achieve uniform dispersion of graphene. Using the method of the present invention, both graphene and Al2O3 can be uniformly dispersed in the copper matrix. On the one hand, the comprehensive performance of the composite material can be significantly improved, and the tensile strength can reach more than 400MPa; on the other hand, it has high electrical conductivity, and the electrical conductivity can reach more than 90%IACS.
[0027] (2) The graphene / Al2O3 / Cu composite material and preparation method described in the present invention improve the intrinsic performance of the reinforcement phase: the present invention uses ammonium bicarbonate as a precipitant, and ammonium bicarbonate and aluminum salt can generate ammonium aluminum carbonate. It is not easy to generate hydrogen bonds between ammonium aluminum carbonate powders, and the powders will not agglomerate and grow. At the same time, ammonium aluminum carbonate can be further obtained into smaller powders through thermal decomposition. Therefore, the Al2O3 prepared by the method of the present invention is not only evenly dispersed, but also its size can be precisely controlled to the nanometer level. The present invention adopts an in-situ autogenous method to prepare graphene, and there is no need to modify the graphene. Therefore, the high conductivity of graphene is retained to the greatest extent.
[0028] (3) The graphene / Al2O3 / Cu composite material and preparation method described in the present invention adopts a spray drying method after coprecipitation instead of suction filtration. On the one hand, during the granulation process, the sucrose and polyvinyl alcohol in the solution can be completely retained in the granulated powder and evenly dispersed, thereby ensuring the uniformity of the dispersion of the in-situ self-generated graphene. On the other hand, during the spray drying process, the water evaporates quickly, so that the Al2O3 / Cu obtained by coprecipitation can maintain the uniformity of its composition, and at the same time, it can also prevent the hard agglomeration of the powder formed during the slow drying process.
[0029] (4) The graphene / Al2O3 / Cu composite material and preparation method described in the present invention only require three steps: co-precipitation, high-temperature catalysis, and densification to obtain a graphene / Al2O3 / Cu composite material with uniform dispersion and excellent comprehensive performance. The method is easy to operate, has a simple flow, and a controllable process, and can be repeatedly prepared in batches. It is an efficient, low-cost, batch preparation method for graphene / Al2O3 / Cu composite materials. DETAILED DESCRIPTION
[0030] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The descriptions of "first", "second", etc. mentioned in the embodiments of the present invention are only for descriptive purposes, and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0031] The present invention will be described in detail below with reference to embodiments.
[0032] A method for preparing a dispersion-strengthened copper-graphene composite material, the preparation method comprising the following steps:
[0033] S1. Co-precipitation: copper sulfate Cu(NO3)2 and ammonium aluminum sulfate NH4Al(SO4)2·12H2O are used to prepare a reaction mother liquor, ammonium bicarbonate NH4HCO3 is used to prepare a precipitant, polyvinyl alcohol and sucrose are added to the reaction mother liquor, and the precipitant is added after stirring evenly. After the addition is completed, the reaction is continued for 2 hours to obtain a mixed solution, the mixed solution is stirred evenly, and then spray granulation is performed to obtain granulated powder; the granulated powder is placed in a reduction furnace, and argon gas is first introduced for calcination; and hydrogen gas is then introduced for reduction to obtain Al2O3 / Cu / carbon source mixed powder;
[0034] S2, high temperature catalysis: put the Al2O3 / Cu / carbon source mixed powder into a tube furnace, evacuate, then introduce argon and hydrogen, heat to 800°C, keep warm for 1 to 100 minutes, and then quickly cool to room temperature to obtain graphene / Al2O3 / Cu composite powder;
[0035] S3. Densification: hot pressing and sintering the graphene / Al2O3 / Cu composite powder to obtain a graphene / Al2O3 / Cu composite material.
[0036] The preparation method of the graphene / Al2O3 / Cu composite material of the present invention, steps S1 to S3 are interrelated, and the Al2O3 / Cu / carbon source mixed powder is prepared by the coprecipitation method in step S1 to ensure the uniform dispersion of Al2O3 in Cu; at the same time, soluble carbon source sucrose is introduced in the coprecipitation process to provide a carbon source for the subsequent preparation of graphene, so that the carbon source is uniformly dispersed in the Cu matrix, thereby ensuring that the final carbon source catalytically grows on the surface of the copper powder to obtain uniformly dispersed graphene. The uniform dispersion of graphene can be achieved through step S1, and the uniform dispersion of aluminum oxide can also be achieved through the coprecipitation method, effectively improving the strengthening effect of aluminum oxide and graphene. Then, through step S2, high temperature catalysis is performed to grow graphene in situ on the surface of the copper powder to achieve uniform dispersion of graphene; the graphene is prepared by an in-situ self-generated method, and there is no need to modify the graphene, so the high electrical conductivity and high thermal conductivity of graphene are retained to the greatest extent; finally, the graphene / Al2O3 / Cu composite powder is hot-pressed and sintered through S3 to obtain a graphene / Al2O3 / Cu composite material. Using the method of the present invention, first, both graphene and Al2O3 can be uniformly dispersed in the copper matrix; second, the comprehensive performance of the composite material can be significantly improved, and the tensile strength can reach more than 400MPa; third, it has high electrical conductivity, and the conductivity can reach more than 90%IACS; fourth, it has high density, few defects, and uniform microstructure.
[0037] Specifically, in step S1, the concentration of copper sulfate is 0.5-2 mol / L, the concentration of ammonium aluminum sulfate is 0.001-0.03 mol / L, and the ratio of ammonium aluminum sulfate to copper sulfate is calculated according to the mass fraction of Al2O3 in Cu produced in the end.
[0038] Specifically, in step S1, the concentration of the ammonium bicarbonate solution is 0.1-2 mol / L.
[0039] Specifically, in step S1, ammonium bicarbonate NH4HCO3 is used to prepare a precipitant, and the pH value is adjusted to 7-12 with ammonia water.
[0040] Specifically, in step S1, before adding polyvinyl alcohol and sucrose to the reaction mother solution, the temperature of the mother solution is controlled at 10-90°C.
[0041] Specifically, in step S1, sucrose is used as a carbon source to provide a carbon source for preparing graphene in step S2, and the amount of sucrose added is 0.6-8 g / L, and the specific content is adjusted according to the copper ion concentration and the graphene content.
[0042] Specifically, in step S1, polyvinyl alcohol (PVA) is used as a dispersant to avoid agglomeration during the coprecipitation process and to make the powder dispersed evenly. The amount of PVA added is 0.5 to 15 g / L. PVA also provides a carbon source for preparing graphene in step S2.
[0043] Specifically, in step S1, a precipitant is added to the reaction mother solution at a rate of 5 to 1000 ml / min. When the pH value of the final reaction solution reaches 7 to 10, the addition of the precipitant can be stopped.
[0044] Specifically, in step S1, the mixed solution is stirred evenly, and then granulated using a spray granulation tower. In this way, sucrose and polyvinyl alcohol (PVA) can be completely retained in the granulated powder. At the same time, during the granulation process, sucrose and PVA can be evenly dispersed in the powder, thereby ensuring the uniformity of the in-situ self-generated graphene. The reaction byproduct in the solution is mainly ammonium nitrate, which can be decomposed during the later calcination process.
[0045] Specifically, in step S1, the spray granulation process is: inlet air temperature 100-300°C, outlet air temperature 60-200°C, atomizer frequency 20-50Hz.
[0046] Specifically, in step S1, calcination is carried out in an argon atmosphere, and the calcination process is: firstly heating to 250°C and keeping the temperature for 4 hours to fully decompose the ammonium nitrate; then heating to 400-500°C and keeping the temperature for 1-6 hours.
[0047] Specifically, in step S1, the reduction is carried out in a hydrogen atmosphere, and the reduction process is: the temperature is 400-500° C., and the insulation time is 1-6 hours.
[0048] Specifically, in step S2, the flow rate of argon gas is 10-500 ml / min, and the flow rate of hydrogen gas is 10-500 ml / min.
[0049] Specifically, in step S3, the hot pressing sintering process is: pressure 30-50 MPa, temperature 750-950° C., and heat preservation time 1-10 hours.
[0050] Example 1
[0051] This embodiment provides a method for preparing a graphene / Al2O3 / Cu composite material, and the preparation method comprises the following steps:
[0052] The preparation method comprises the following steps:
[0053] S1. Co-precipitation: copper sulfate Cu(NO3)2 and ammonium aluminum sulfate NH4Al(SO4)2·12H2O are used to prepare a reaction mother liquor, and ammonium bicarbonate NH4HCO3 is used to prepare a precipitant, polyvinyl alcohol and sucrose are added to the reaction mother liquor, and the precipitant is added after stirring evenly. After the addition is completed, the reaction is continued for 2 hours to obtain a mixed solution, and the mixed solution is stirred evenly and then spray granulated to obtain granulated powder; the granulated powder is placed in a reduction furnace, first evacuated, and argon gas is introduced for calcination; and then evacuated, and hydrogen gas is introduced for reduction to obtain Al2O3 / Cu / carbon source mixed powder;
[0054] S2, high temperature catalysis: put the Al2O3 / Cu / carbon source mixed powder into a tube furnace, evacuate, then introduce argon and hydrogen, heat to 800°C, keep warm for 20 minutes, and then quickly cool to room temperature to obtain graphene / Al2O3 / Cu composite powder;
[0055] S3. Densification: hot pressing and sintering the graphene / Al2O3 / Cu composite powder to obtain a graphene / Al2O3 / Cu composite material.
[0056] Specifically, in step S1, 3800 g of Cu(NO3)2 and 22 g of NH4Al(SO4)2·12H2O are added to 10 L of pure water, and mechanical stirring is started, and a reaction mother solution is prepared after the two are dissolved.
[0057] In step S1, the concentration of copper sulfate is 2 mol / L, the concentration of ammonium aluminum sulfate is 0.004 mol / L, and the concentration of ammonium bicarbonate solution is 1.35 mol / L.
[0058] In step S1, ammonium bicarbonate NH4HCO3 is used to prepare a precipitant, and the pH value is adjusted to 11 with aqueous ammonia.
[0059] Specifically, in step S1, 3200 g of NH4HCO3 is added to 30 L of pure water, and then ammonia water is added, and the pH value is adjusted to 11 to prepare a precipitant.
[0060] Specifically, in step S1, before adding polyvinyl alcohol and sucrose to the reaction mother liquor, the temperature of the mother liquor is controlled at 40°C; then 250g of 10% PVA solution is added, and then 20g of sucrose is added.
[0061] Specifically, in step S1, a precipitant is added to the reaction mother solution at a rate of 80 ml / min. When the pH value of the final reaction solution reaches 9, the addition of the precipitant can be stopped.
[0062] Specifically, in step S1, the spray granulation process is: inlet air temperature 180°C, outlet air temperature 90°C, and atomizer frequency 30 Hz.
[0063] Specifically, in step S1, calcination is carried out in an argon atmosphere, and the calcination process is: firstly heating to 250°C and keeping the temperature for 4 hours to fully decompose the ammonium nitrate; then heating to 500°C and keeping the temperature for 3 hours.
[0064] Specifically, in step S1, the reduction is performed under a hydrogen atmosphere, and the reduction process is: the temperature is 500° C., and the insulation time is 5 hours.
[0065] Specifically, in step S2, the Al2O3 / Cu / carbon source mixed powder is placed in a tubular furnace, evacuated to 80Pa, and then argon and hydrogen are introduced, with the argon flow rate being 200ml / min and the hydrogen flow rate being 50ml / min; the temperature is raised to 800°C, kept warm for 20 minutes, and then quickly cooled to room temperature by air cooling to obtain graphene / Al2O3 / Cu composite powder.
[0066] Specifically, in step S3, the graphene / Al2O3 / Cu composite powder is placed in a hot pressing sintering furnace for densification to obtain a graphene / Al2O3 / Cu composite material. The hot pressing sintering process is: pressure 50 MPa, temperature 750°C, and insulation for 10 hours.
[0067] Example 2
[0068] Different from Example 1, in this embodiment,
[0069] Specifically, in step S1, 3800 g of Cu(NO3)2 and 50 g of NH4Al(SO4)2·12H2O are added to 10 L of pure water, and mechanical stirring is started, and a reaction mother solution is prepared after the two are dissolved.
[0070] In step S1, the concentration of copper sulfate is 2 mol / L, the concentration of ammonium aluminum sulfate is 0.01 mol / L, and the concentration of ammonium bicarbonate solution is 1.35 mol / L.
[0071] In step S1, ammonium bicarbonate NH4HCO3 is used to prepare a precipitant, and the pH value is adjusted to 10 with aqueous ammonia.
[0072] Specifically, in step S1, 3200 g of NH4HCO3 is added to 30 L of pure water, and then ammonia water is added, and the pH value is adjusted to 10 to prepare a precipitant.
[0073] Specifically, in step S1, before adding polyvinyl alcohol and sucrose to the reaction mother liquor, the temperature of the mother liquor is controlled at 70°C; then 300g of 10% PVA solution is added, and then 15g of sucrose is added.
[0074] Specifically, in step S1, a precipitant is added to the reaction mother solution at a rate of 120 ml / min. When the pH value of the final reaction solution reaches 7.5, the addition of the precipitant can be stopped.
[0075] Specifically, in step S1, the spray granulation process is: inlet air temperature 220°C, outlet air temperature 100°C, and atomizer frequency 50 Hz.
[0076] Specifically, in step S1, calcination is carried out in an argon atmosphere, and the calcination process is: firstly heating to 250°C and keeping the temperature for 4 hours to fully decompose the ammonium nitrate; then heating to 450°C and keeping the temperature for 3 hours.
[0077] Specifically, in step S1, the reduction is performed under a hydrogen atmosphere, and the reduction process is: the temperature is 450° C., and the insulation time is 5 hours.
[0078] Specifically, in step S2, the argon flow rate is 200 ml / min, and the hydrogen flow rate is 80 ml / min.
[0079] Specifically, in step S3, the hot pressing sintering process is: pressure 30 MPa, temperature 950° C., and heat preservation for 1 hour.
[0080] Example 3
[0081] This embodiment proposes a graphene / Al2O3 / Cu composite material, which is prepared using the preparation method of the graphene / Al2O3 / Cu composite material as described in any one of Embodiment 1 or Embodiment 2.
[0082] The advantages of the graphene / Al2O3 / Cu composite material and the preparation method of the graphene / Al2O3 / Cu composite material mentioned above over the prior art are the same, which will not be repeated here.
[0083] Comparative Example 1
[0084] In this comparative example, the same Al2O3 content and graphene content as those in Example 1 are used; different from Example 1, the preparation method described in the patent application number CN201810014534.8 is adopted for preparation.
[0085] Performance Testing
[0086] The performance of the graphene / Al2O3 / Cu composite materials prepared in Examples 1 to 2 and Comparative Example 1 was tested, and the test results are shown in Table 1.
[0087] Table 1
[0088]
[0089] It can be seen from Table 1 that the graphene / Al2O3 / Cu composite materials prepared in Examples 1 to 2 of the present invention can significantly improve the comprehensive properties of the composite materials, with a tensile strength of more than 412 MPa; and have high electrical conductivity, with an electrical conductivity of more than 90% IACS.
[0090] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A graphene / Al 2 O 3 Preparation method of / Cu composite material, It is characterized in that The preparation method comprises the following steps: S1. Coprecipitation: using copper sulfate Cu(NO 3 ) 2 and ammonium aluminum sulfate NH 4 Al(SO 4 ) 2 12H 2 O to prepare the reaction mother solution, using ammonium bicarbonate NH 4 HCO 3 Prepare a precipitant, add polyvinyl alcohol and sucrose to the reaction mother liquor, stir evenly and then add the precipitant, after the addition is complete, continue the reaction for 2 hours to obtain a mixed solution; spray granulate the mixed solution to obtain granulated powder; put the granulated powder into a reduction furnace, first calcine it, and then reduce it to obtain Al 2 O 3 / Cu / carbon source mixed powder; S2, high temperature catalysis: Al 2 O 3 The mixed powder of Al / Cu / carbon source was placed in a tube furnace, vacuumed, and then argon and hydrogen were introduced. The temperature was raised to 800°C, kept at this temperature for 1 to 100 minutes, and then quickly cooled to room temperature to obtain graphene / Al 2 O 3 / Cu composite powder; S3. Densification: Graphene / Al 2 O 3 / Cu composite powder is hot pressed and sintered to obtain graphene / Al 2 O 3 / Cu composite materials.
2. A graphene / Al according to claim 1 2 O 3 Preparation method of / Cu composite material, It is characterized in that In step S1, before adding polyvinyl alcohol and sucrose to the reaction mother liquor, the temperature of the mother liquor is controlled at 10-90°C.
3. A graphene / Al according to claim 2 2 O 3 Preparation method of / Cu composite material, It is characterized in that In step S1, a precipitant is added to the reaction mother solution at a rate of 5 to 1000 ml / min. When the pH value of the final reaction solution reaches 7 to 10, the addition of the precipitant can be stopped.
4. A graphene / Al according to claim 3 2 O 3 Preparation method of / Cu composite material, It is characterized in that In step S1, the spray granulation process is: inlet air temperature 100-300°C, outlet air temperature 60-200°C, atomizer frequency 20-50Hz.
5. A graphene / Al according to claim 4 2 O 3 Preparation method of / Cu composite material, It is characterized in that In step S1, calcination is carried out in an argon atmosphere, and the calcination process is: firstly heating to 250°C and keeping the temperature for 4 hours to fully decompose the ammonium nitrate; then heating to 400-500°C and keeping the temperature for 1-6 hours.
6. A graphene / Al according to claim 5 2 O 3 Preparation method of / Cu composite material, It is characterized in that In step S1, the reduction is carried out in a hydrogen atmosphere, and the reduction process is as follows: the temperature is 400-500° C., and the insulation time is 1-6 hours.
7. The graphene / Al according to claim 1 2 O 3 Preparation method of / Cu composite material, It is characterized in that In step S2, the flow rate of argon gas is 10 to 500 ml / min, and the flow rate of hydrogen gas is 10 to 500 ml / min.
8. The graphene / Al according to claim 1 2 O 3 Preparation method of / Cu composite material, It is characterized in that In step S3, the hot pressing sintering process is: pressure 30-50 MPa, temperature 750-950° C., and heat preservation time 1-10 hours.
9. The graphene / Al according to claim 1 2 O 3 Preparation method of / Cu composite material, It is characterized in that In step S1, ammonium bicarbonate NH 4 HCO 3 Prepare the precipitant and adjust the pH value to 7-12 with ammonia water.
10. A graphene / Al 2 O 3 / Cu composite materials, It is characterized in that The graphene / Al 2 O 3 The graphene / Al / Cu composite material uses the graphene / Al / Cu composite material according to any one of claims 1 to 9. 2 O 3 / Cu composite material is prepared by a preparation method.
Citation Information
Cited By
Graphene reinforced Al-Cu composite material and preparation method