Hierarchical porous carbon composite tin-antimony alloy materials for alkali metal ion secondary batteries
In the preparation of alkali metal ion secondary battery negative electrode materials, ball milling and high-temperature sintering processes are used to form a graded porous carbon composite tin antimony alloy material, which solves the problems of complex process, high cost and insufficient performance in the prior art, and achieves high capacity , electrochemical properties of cycle stability and safety.
Patent Information
- Application Number
- CN202411226890.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The prior art when preparing alkali metal ion secondary battery negative electrode materials, the process is complex and the cost is high, and the circulation and rate performance of the material are insufficient, making it difficult to meet the needs of high specific energy, fast charging and safety.
The organic metal salt containing tin and alkali metal and the organic metal salt containing antimony and alkali metal are mixed for ball milling, and sintered at high temperature in a reducing atmosphere to form a composite of antimony tin alloy and water-soluble carbonate, which is retained by washing and dissolution process. The rich multi-stage porous structure is used to prepare a graded porous carbon composite tin antimony alloy material.
It realizes the preparation of high-performance negative electrode materials with simple process and low cost. The materials show excellent electrochemical properties in lithium, sodium and potassium ion secondary batteries, including high capacity, cycling performance and rate performance, and the working voltage is suitable and safe. Highly sexual.
Smart Images

Figure CN118720158B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to electrode materials for alkali metal (lithium, sodium, potassium) ion secondary batteries, and specifically relates to a graded porous carbon composite tin-antimony alloy material for alkali metal ion secondary batteries. Background Art
[0002] Under the theme of sustainable development, green energy has been vigorously developed, and at the same time, higher requirements have been put forward for energy storage systems. Among them, lithium-ion secondary batteries have the advantages of high energy density, long service life, and small size, and have been commercially used in portable electronic devices, electric vehicles, and large energy storage devices. However, the natural abundance of lithium resources is low, and the price of lithium ore has continued to rise with the expansion of the battery market, making it difficult to meet the growing demand. Sodium and potassium, which are also alkali metals, have very similar physical and chemical properties to lithium and have very abundant reserves. Therefore, the development and application of sodium-ion batteries and potassium-ion batteries can solve the difficulties faced by lithium-ion batteries today. At present, sodium-ion batteries have achieved initial market-oriented production, and potassium-ion batteries with relatively high working voltages are also gradually advancing towards commercial applications.
[0003] As one of the key components of alkali metal ion secondary batteries, the negative electrode determines the performance of the battery. At present, the main negative electrode active materials used in mainstream applications are carbon materials, among which graphite negative electrodes are used in lithium ion batteries and potassium ion batteries, and hard carbon negative electrodes are used in sodium ion batteries. However, these negative electrodes have problems such as low specific capacity, poor rate performance, and great safety hazards (too low discharge voltage leads to alkali metal precipitation and dendrite growth), which are difficult to meet the current battery market's demand for high specific energy, fast charging, and safety. Among many candidate negative electrode materials, tin and antimony, as metal alloy negative electrode materials, have high specific capacity, excellent rate performance, and suitable discharge voltage, which meet the above requirements and are strong competitors for the next generation of battery negative electrode materials. However, tin and antimony face the problem of poor cycle performance caused by the huge volume change associated with the charging and discharging process, which seriously limits their application. Constructing carbon-composite tin-antimony alloy materials is an effective strategy to improve their cycle stability, because tin-antimony alloys can buffer stress each other by utilizing the different alloying reaction potentials of tin and antimony with alkali metal ions, and the introduction of carbon matrix can buffer stress and maintain an effective conductive path. In addition, introducing a large number of pores into the composite material can provide a buffer space for volume expansion, which is beneficial to the release of stress and thus maintain the integrity of the structure. The abundant pores are also conducive to the infiltration of electrolytes and the transmission of ions, which is very beneficial to the improvement of the battery's cycle performance and rate performance.
[0004] In the "Preparation method and application of SnSb nanoparticles / three-dimensional nitrogen-doped nanoporous carbon composite materials" disclosed in patent CN110190261A, the metal organic framework material ZIF-8 containing Zn is carbonized at high temperature and etched with acid. In this process, the zinc nanoparticles formed by high-temperature carbon thermal reduction are removed by high-temperature volatilization and acid etching, leaving abundant micro / mesopores in the carbon material. Then, the method of reducing tin ions and antimony ions with sodium borohydride is used to introduce tin-antimony alloy nanoparticles into porous carbon to form SnSb nanoparticles / three-dimensional nitrogen-doped nanoporous carbon composite materials. The disadvantage of this process is that the raw material ZIF-8 used is expensive, and the zinc particles are used as templates. A large amount of volatilization during the carbon thermal process is difficult to recover. Furthermore, the process conditions are harsh when preparing alloys by sodium borohydride reduction, and sodium borohydride is an explosive chemical, which is very dangerous. In addition, the loading of porous carbon and tin-antimony alloy in the process is carried out in two steps, which easily leads to some micro / mesopores being occupied by the subsequently introduced alloy particles, significantly reducing the number of pores, and the micro / mesopores with smaller pore sizes have limited buffering effects on volume expansion and promoting ion transport.
[0005] In the patent CN106992292A, "Three-dimensional graphene embedded ultra-small tin-antimony particle materials and preparation and application", a carbon composite tin-antimony alloy material containing a large number of macropores was prepared by spray pyrolysis of a mixture of inorganic tin salt, inorganic antimony salt and organic carbon source and introduction of the template agent sodium chloride. The disadvantage is that the spray drying process equipment is relatively complex, the thermal efficiency is low, and the energy consumption is high; the presence of a large number of macropores in the prepared material provides a smooth transport channel for the electrolyte, but it will greatly reduce the volume energy density.
[0006] Based on this, it is necessary to design and develop a simple and low-cost method to achieve the preparation of graded porous carbon composite tin-antimony alloy materials. Summary of the invention
[0007] Based on the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a graded porous carbon composite tin-antimony alloy material for the negative electrode of an alkali metal ion secondary battery, aiming to obtain a high-performance negative electrode material with a simple process.
[0008] In order to achieve the purpose, the present invention adopts the following technical scheme:
[0009] A preparation method of a hierarchical porous carbon composite tin-antimony alloy material for the negative electrode of an alkali metal ion secondary battery, characterized in that: using organic metal salts containing tin and alkali metals and organic metal salts containing antimony and alkali metals as raw materials, ball milling and mixing them evenly, sintering them at high temperature in a reducing atmosphere to form a composite of antimony-tin alloy, water-soluble carbonate and carbon, and then washing and dissolving the carbonate formed in situ during the sintering process to leave holes to obtain a rich multi-level pore structure, thereby obtaining a hierarchical porous carbon composite tin-antimony alloy material. Specifically comprising the following steps:
[0010] Step 1: Ball milling
[0011] According to the Sn / Sb molar ratio of 1:1, an organic metal salt containing tin and an alkali metal and an organic metal salt containing antimony and an alkali metal are mixed and ball-milled at a ball-milling speed of 200-500 rpm for 2-6 h to obtain a precursor powder;
[0012] Step 2: Reduction sintering
[0013] The precursor powder is sintered at high temperature in a reducing atmosphere, with a gas flow rate of 20-100 sccm, a sintering temperature of 500-600°C, a sintering time of 1-3 h, a heating rate of 2-10°C / min, and a sintered powder is obtained after natural cooling;
[0014] Step 3: Wash and remove the template
[0015] The sintered powder is soaked in deionized water for 1-6 hours, the soaking liquid is filtered out, and then washed with deionized water for at least 3 times. After drying, a graded porous carbon composite tin-antimony alloy material is obtained.
[0016] Furthermore, the organic metal salt containing tin and alkali metal or the organic metal salt containing antimony and alkali metal is composed of organic acid anions (including citrate, tartrate, gluconate, etc.), tin cations or antimony cations, and alkali metal cations (Na + , K + ), some of which contain crystal water, and the general chemical formula is C x H y O z A w B v uH2O, where A is Sn or Sb, B is an alkali metal (Na or K), 0 <x,y,z<20,0<w,v<5,0≤u<10。
[0017] Furthermore, the organic metal salt containing tin and alkali metal is disodium stannous citrate (C6H5O7SnNa2); the organic metal salt containing antimony and alkali metal is potassium antimony oxytartrate trihydrate (C8H4O 12 Sb2K2·3H2O), potassium antimony tartrate hemihydrate (C4H4O7SbK·0.5H2O), sodium antimony L-tartrate (C4H4O7SbNa) and sodium antimony gluconate nonahydrate (C 12 H 17 O 17 Sb2Na3·9H2O), preferably potassium antimony tartrate trihydrate.
[0018] Furthermore, the ball milling is dry ball milling without adding a dispersant or wet ball milling with adding an organic dispersant. After the dry ball milling, the precursor powder is directly obtained, and after the wet ball milling, the precursor powder is obtained by drying; wherein the organic dispersant used in the wet ball milling is one of ethanol, acetone, and cyclohexane. Preferably, acetone is used as a dispersant for wet ball milling, the ball milling speed is 200 rpm, the ball milling time is 2 h, and after completion, it is dried in an oven at 60°C.
[0019] Furthermore, the reducing atmosphere is at least one of hydrogen, argon-hydrogen mixed gas, and nitrogen-hydrogen mixed gas.
[0020] Furthermore, in the above-mentioned preparation method of the present invention: during the high-temperature sintering process in a reducing atmosphere, the organic ligands in the mixed organic metal salt are pyrolyzed to form a carbon skeleton, the alkali metal ions are converted into water-soluble carbonates (sodium carbonate, potassium carbonate) as templates, and the tin ions and antimony ions are reduced to elemental substances and in situ form tin-antimony alloy nanoparticles, which are encapsulated in the carbon matrix to form a composite.
[0021] The hierarchical porous carbon composite tin-antimony alloy material prepared by the present invention has tin-antimony alloy particles with a particle size of 10-50 nm embedded in a hierarchical porous carbon skeleton to form a three-dimensional composite structure with an overall size of 1-10 μm, and the mass fraction of the alloy in the composite material is 78%-81%. The material can be generally used in alkali metal (lithium, sodium, potassium) ion secondary batteries, with suitable working potential, high capacity, excellent cycle performance and rate performance.
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0023] The present invention is composed of organic acid anions, tin cations and alkali metal cations (Na + , K + ) and organic metal salts composed of organic acid anions, antimony cations and alkali metal cations (Na + , K + ) as raw materials, the two salts are ball-milled and mixed evenly, and then pyrolyzed in a reducing atmosphere to form a composite of tin-antimony alloy, water-soluble carbonate (sodium carbonate, potassium carbonate) and carbon, wherein the carbonate template formed in situ is washed and dissolved with water, leaving abundant holes, and a graded porous carbon composite tin-antimony alloy material is prepared. The process of the present invention is simple and the cost is low. The ball milling equipment and atmosphere furnace used in the process are commonly used equipment in industrial production, and are suitable for industrial large-scale production.
[0024] In the hierarchical porous carbon composite tin-antimony alloy material developed by the present invention, nanoscale tin-antimony alloy particles are embedded in a hierarchical porous carbon skeleton, and the carbon skeleton can effectively limit the agglomeration of alloy particles, buffer the stress of alloy particles during volume changes caused by electrochemical cycles, and provide a smooth conductive path; the presence of hierarchical porosity can provide a buffer space for the repeated volume expansion / contraction of alloy particles to maintain the integrity of the structure, and is beneficial to the infiltration of electrolyte and the transmission of ions. The material exhibits excellent electrochemical properties in lithium ion, sodium ion and potassium ion secondary batteries: it has a low and safe operating voltage in the three types of ion secondary batteries; in lithium ion batteries, after 400 cycles at a current density of 1 A / g, the capacity is as high as 552 mAh / g, with a capacity retention rate of 90%, and the specific capacity is as high as 710 mAh / g at a current density of 0.1 A / g, and the specific capacity is as high as 393 mAh / g at a high current density of 10 A / g; as the negative electrode of sodium ion batteries, after 300 cycles at a current density of 1 A / g, the capacity reaches 292 mAh / g, with a capacity retention rate of 92%, and the specific capacity reaches 187 mAh / g at a high current density of 10 A / g; in potassium ion batteries, after 500 cycles at a current density of 0.5 A / g, the capacity reaches 317 mAh / g, with almost no capacity decay, and the capacity is still 260 mAh / g after 500 cycles at a current density of 1 A / g, showing a wide range of application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a scanning electron microscope image of the precursor powder in Example 1 of the present invention.
[0026] Figure 2 This is a scanning electron microscope image of the sintered powder in Example 1 of the present invention.
[0027] Figure 3 This is the X-ray diffraction pattern of the finished powder (SSC) in Example 1 of the present invention.
[0028] Figure 4 This is a scanning electron microscope image of the finished powder (SSC) in Example 1 of the present invention, where (a) and (b) correspond to different magnifications.
[0029] Figure 5 This is a transmission electron microscope image of the finished powder (SSC) in Example 1 of the present invention.
[0030] Figure 6 This is the scanning electron microscope (SEM) of the finished powder (SSC) in Example 1 of the present invention. Figure 6 (a)) and carbon ( Figure 6 (b) in), tin ( Figure 6 (c)), antimony ( Figure 6 Element distribution diagram in (d).
[0031] Figure 7 This is the X-ray diffraction pattern of the finished powder (SSC-500°C) in Example 2 of the present invention.
[0032] Figure 8 This is a scanning electron microscope image of the finished powder (SSC-500°C) in Example 2 of the present invention.
[0033] Fig. 9 1 and 2 are X-ray diffraction patterns of SnC in Comparative Example 1 and SbC in Comparative Example 2 of the present invention.
[0034] Fig.10 This is a scanning electron microscope image of SnC in comparative example 1 of the present invention, wherein (a) and (b) correspond to different magnifications.
[0035] Fig.11 This is a scanning electron microscope image of SbC in comparative example 2 of the present invention, wherein (a) and (b) correspond to different magnifications.
[0036] Fig.12 The nitrogen adsorption-desorption curves and specific surface areas of the finished powder (SSC) in Example 1 of the present invention, the SnC in Comparative Example 1, and the SbC in Comparative Example 2 are shown.
[0037] Fig.13 This is the charge and discharge curve when the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention is used as the negative electrode of a lithium-ion battery.
[0038] Fig.14 The cycle performance of the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention when used as a negative electrode of a lithium-ion battery is compared with that of SnC in Comparative Example 1 and SbC in Comparative Example 2.
[0039] Fig.15 The figure is the rate performance of the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention when used as the negative electrode of a lithium-ion battery.
[0040] Fig.16 1 is a charge and discharge curve of the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention when used as the negative electrode of a sodium ion battery.
[0041] Fig.17 The cycle performance of the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention when used as a negative electrode of a sodium ion battery is compared with that of SnC in Comparative Example 1 and SbC in Comparative Example 2.
[0042] Fig.18 The figure is the rate performance of the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention when used as the negative electrode of a sodium ion battery.
[0043] Fig.19 This is the charge and discharge curve when the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention is used as the negative electrode of a potassium ion battery.
[0044] Fig. 20 The hierarchical porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention is used as the negative electrode of a potassium ion battery at 0.5 A g -1 Cycling performance at different current densities.
[0045] Fig.21 The cycle performance of the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 of the present invention when used as the negative electrode of a potassium ion battery is compared with that of SnC in Comparative Example 1 and SbC in Comparative Example 2.
[0046] Fig. 22 It is the X-ray diffraction pattern of SSC-12 in Comparative Example 3 of the present invention.
[0047] Fig.23 This is a scanning electron microscope image of SSC-12 in Comparative Example 3 of the present invention.
[0048] Fig.24 The SEM of SSC-12 in Comparative Example 3 of the present invention ( Fig.24 (a)) and carbon ( Fig.24 (b) in), tin ( Fig.24 (c)), antimony ( Fig.24 Element distribution diagram in (d).
[0049] Fig.25 This is the X-ray diffraction pattern of SSC-700°C in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. However, the accompanying drawings and embodiments do not constitute a limitation on the technical solution of the present invention.
[0051] Example 1
[0052] Disodium stannous citrate (C6H5O7SnNa2) and potassium antimony tartrate trihydrate (C8H4O 12 Sb2K2·3H2O) was dispersed in acetone dispersant at a Sn / Sb molar ratio of 1:1, with a solid content of 30%. The mixture was ball-milled at a speed of 200 rpm for 2 h, and the ball-milled product was placed in a 60°C forced air oven for 12 h to remove the acetone dispersant, to obtain a precursor powder, such as Figure 1 As shown, its morphology is micron-scale agglomerates composed of irregular nanoparticles.
[0053] The prepared precursor powder was calcined in an argon-hydrogen mixed gas (hydrogen content of 5%) with a gas flow rate of 60 sccm, heated to 600°C at a heating rate of 3°C / min for 2 h, and then naturally cooled to room temperature to obtain a sintered powder. Figure 2 As shown, the sintered powder is a composite of antimony-tin alloy nanoparticles, sodium carbonate, potassium carbonate and carbon.
[0054] The sintered powder was soaked in deionized water for 1 h. During this process, the sodium carbonate and potassium carbonate used as templates in the composite structure dissolved in the water, leaving holes in the composite material. The soaking liquid was then removed by filtration, washed three times with deionized water, and dried in a vacuum oven at 80°C to obtain the finished powder, i.e., graded porous carbon composite tin-antimony alloy material (SSC). It was subjected to X-ray diffraction test, scanning electron microscopy test, transmission electron microscopy test, energy dispersive X-ray spectroscopy element distribution test, and nitrogen adsorption and desorption test.
[0055] Figure 3 The X-ray diffraction pattern of the finished powder is in good agreement with the standard pattern of tin-antimony alloy; Figure 4 The scanning electron microscope images show that the micron-sized particles have an obvious hierarchical porous structure, in which the tin-antimony alloy particles are well embedded in the carbon skeleton; Figure 5 The transmission electron microscope image shows that the tin-antimony alloy nanoparticles are about 50 nm in size and are perfectly wrapped by the carbon matrix; Figure 6 The element distribution diagram shows the uniform distribution of carbon, tin and antimony in the composite material. Fig.12 The nitrogen adsorption and desorption curve of SSC is shown, and its specific surface area is 98.3 m 2 g -1 .
[0056] Example 2
[0057] Disodium stannous citrate (C6H5O7SnNa2) and potassium antimony tartrate trihydrate (C8H4O 12Sb2K2·3H2O) was dispersed in acetone dispersant with a Sn / Sb molar ratio of 1:1, with a solid content of 30%. The mixture was ball-milled at a speed of 200rpm for 2 h, and the ball-milled product was placed in a 60℃ forced air oven for 12 h to remove the acetone dispersant to obtain a precursor powder. The prepared precursor powder was calcined in an argon-hydrogen mixed gas (hydrogen content was 5%) with a gas flow rate of 60sccm, and the temperature was raised to 500℃ for 2 h at a heating rate of 3℃ / min, and then naturally cooled to room temperature to obtain a sintered powder. The sintered powder was soaked in deionized water for 1 h. During this process, the sodium carbonate and potassium carbonate used as templates in the composite structure dissolved in the water, leaving pores in the composite material. After that, the soaking liquid was separated and removed by suction filtration, washed with deionized water three times, and dried in a vacuum oven at 80℃ to obtain the finished powder SSC-500℃. It was tested by X-ray diffraction and scanning electron microscopy.
[0058] Figure 7 The X-ray diffraction pattern of the finished powder SSC-500℃ is in good agreement with the standard pattern of tin-antimony alloy; Figure 8 The scanning electron microscope images show that the micron-sized particles have an obvious hierarchical porous structure, in which the tin-antimony alloy particles are well embedded in the carbon skeleton.
[0059] Comparative Example 1
[0060] The difference from Example 1 is that the tin-containing salt disodium stannous citrate (C6H5O7SnNa2) is dispersed in the acetone dispersant, and the other parts are kept the same to obtain a tin-carbon composite material (SnC). X-ray diffraction test, scanning electron microscope test and nitrogen adsorption-desorption test are performed on it.
[0061] Fig. 9 The X-ray diffraction pattern of SnC in the sample is in good agreement with the standard pattern of tin metal; Fig.10 The scanning electron microscope image shows that the micron-sized particles have a porous structure, among which the tin particles are relatively large, about 500 nm in size. Fig.12 The nitrogen adsorption and desorption curve of SnC is shown. The specific surface area of SnC is 97.8 m 2 g -1 .
[0062] Comparative Example 2
[0063] The difference from Example 1 is that the antimony-containing salt potassium antimony oxytartrate trihydrate (C8H4O 12 Sb2K2·3H2O) was dispersed in acetone dispersant, and other components were kept the same to obtain antimony carbon composite material (SbC). It was tested by X-ray diffraction, scanning electron microscopy and nitrogen adsorption-desorption.
[0064] Fig. 9The X-ray diffraction pattern of SbC in the sample is in good agreement with the standard pattern of antimony metal; Fig.11 The scanning electron microscope image shows that the micron-sized particles have a porous structure. The antimony particles are about 300 nm in size. Some antimony particles are accumulated and exposed outside the carbon skeleton and fail to composite well with the carbon skeleton. Fig.12 The nitrogen adsorption-desorption curve of SbC is shown. The specific surface area of SbC is 59.2 m 2 g -1 .
[0065] From the above comparison, it can be seen that the nanoscale (about 50 nm) tin-antimony alloy particles in the hierarchical porous carbon composite tin-antimony alloy material (SSC) prepared in Example 1 are embedded in the hierarchical porous carbon skeleton. In contrast, there are many tin particles with larger particle sizes (about 500 nm) in the tin-carbon composite material (SnC) prepared using a single tin salt in Comparative Example 1. The antimony particles in the antimony-carbon composite material (SbC) prepared using a single antimony salt in Comparative Example 2 are about 300 nm in size, and some antimony particles are accumulated and exposed outside the carbon skeleton. By comparison, it can be found that the present invention can greatly improve the problem of large single metal particle size and poor compounding with the carbon skeleton. Reducing the particle size is conducive to maintaining the integrity of the structure of the particles during volume change and improving the rate performance; good compounding of metal particles with carbon matrix is conducive to buffering the stress of particle volume change and maintaining a good conductive path. In addition, SSC exhibits the largest specific surface area, indicating that it has a very rich pore, which can provide a buffer space for repeated volume expansion / contraction of alloy particles to maintain the integrity of the structure, and is conducive to the infiltration of electrolytes and the transmission of ions.
[0066] The electrochemical performance of the graded porous carbon composite tin-antimony alloy material (SSC) in Example 1 and the tin-carbon composite material (SnC) and antimony-carbon composite material (SbC) in Comparative Examples 1-2 was tested by the following method:
[0067] The prepared negative electrode material was mixed with acetylene black and sodium carboxymethyl cellulose in a mass ratio of 7:2:1 with water as a dispersant to form a slurry, and then the slurry was coated on a copper foil by a doctor blade casting method and dried in a vacuum oven at 60°C for 8 hours. After drying, it was punched into discs with a diameter of 10 mm, in which the active material loading was about 1 mg / cm 2 .
[0068] The prepared electrode sheets were used to assemble CR2032 button batteries, specifically: the lithium-ion battery used a lithium sheet as a counter electrode, the electrolyte was 1 mol / L lithium hexafluorophosphate dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1, 5% by volume of fluoroethylene carbonate (FEC) was added as an additive, and a Celgard 2400 model separator was used; the sodium-ion battery used a sodium metal sheet as a counter electrode, the electrolyte was 1 mol / L sodium hexafluorophosphate dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1, 5% by volume of fluoroethylene carbonate (FEC) was added as an additive, and glass fiber was used as a separator; the potassium-ion battery used a potassium metal sheet as a counter electrode, the electrolyte was 5 mol / L potassium bis(fluorosulfonyl)imide (KFSI) dissolved in ethylene glycol dimethyl ether (DME), and glass fiber was used as a separator.
[0069] Constant current charge and discharge test was performed using the assembled alkali metal ion half-cell: Fig.13 , Fig.16 and Fig.19 These are the charge and discharge curves of the SSC in Example 1 at a current density of 0.1 A / g in lithium ion, sodium ion and potassium ion batteries, respectively, all of which have a relatively low and safe operating voltage. Fig.14 and Fig.15 The electrochemical performance of SSC in lithium-ion batteries shows that its capacity is as high as 552 mAh / g after 400 cycles at a current density of 1 A / g in lithium-ion batteries, and the capacity retention rate is 90% ( Fig.14 ), the cycle stability is significantly better than that of SnC in Comparative Example 1 and SbC in Comparative Example 2. The specific capacity of SSC at a current density of 0.1 A / g is as high as 710 mAh / g, and the specific capacity at a high current density of 10 A / g is as high as 393 mAh / g ( Fig.15 ), showing excellent rate performance. Fig.17 and Fig.18 The electrochemical performance of SSC in sodium ion batteries is shown in Figure 2. As the negative electrode of sodium ion batteries, it can be stably cycled for 400 cycles at a current density of 1 A / g, and the capacity retention rate is 81% ( Fig.17 ), which is significantly better than SnC in Comparative Example 1 and SbC in Comparative Example 2. SSC has a specific capacity of 187 mAh / g at a high current density of 10 A / g, and also exhibits excellent rate performance ( Fig.18 ). Fig. 20 and Fig.21 The electrochemical performance of SSC in potassium ion batteries is shown in Figure 2. After 500 cycles at a current density of 0.5 A / g in potassium ion batteries, the capacity reaches 317 mAh / g, with almost no capacity decay. Fig.21As shown in the figure, at a high current density of 1 A / g, SSC has both high specific capacity and excellent cycle stability compared with SnC and SbC.
[0070] Comparative Example 3
[0071] The difference from Example 1 is that the Sn / Sb feed ratio is changed: disodium stannous citrate (C6H5O7SnNa2) and potassium antimony tartrate trihydrate (C8H4O 12 Sb2K2·3H2O) was dispersed in acetone dispersant with a Sn / Sb molar ratio of 1:2, and the other parts were kept the same to obtain a finished powder, which was recorded as SSC-12. It was subjected to X-ray diffraction test, scanning electron microscopy test and energy dispersive X-ray spectroscopy element distribution test.
[0072] Fig. 22 The X-ray diffraction pattern of SSC-12 in the sample is in good agreement with the standard pattern of tin-antimony alloy; Fig.23 The SEM images of the particles show two different morphologies: one is micron-sized particles with a hierarchical porous structure, and the other is smooth, non-porous micron-sized blocks. Fig.24 The energy dispersive X-ray spectroscopy element distribution shows that carbon, tin and antimony are evenly distributed on the micron-sized particles with hierarchical porous structure, while the smooth and non-porous micron-sized blocks only show the signals of tin and antimony, indicating that the smooth and non-porous micron-sized blocks are tin-antimony alloy blocks. This means that a large amount of micron-sized tin-antimony alloy does not form a composite structure with carbon.
[0073] Comparative Example 4
[0074] The difference from Example 1 is that the sintering temperature of the precursor powder is raised to 700° C., and the other conditions remain the same, to obtain a finished powder, which is recorded as SSC-700° C. An X-ray diffraction test is performed on the finished powder.
[0075] Fig.25 There are tin-antimony alloy phase and tin metal phase in the X-ray diffraction pattern of SSC-700℃, which means that pure phase tin-antimony alloy material cannot be synthesized by sintering the precursor powder at 700℃.
[0076] Comparative Examples 3 and 4 illustrate that the precursor feed ratio and the sintering temperature are critical for the synthesis of graded porous carbon composite tin-antimony alloy materials (SSC).
[0077] The above are merely exemplary embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a hierarchical porous carbon composite tin-antimony alloy material for an alkali metal ion secondary battery, characterized in that: An organic metal salt containing tin and an alkali metal and an organic metal salt containing antimony and an alkali metal are used as raw materials, ball-milled and mixed evenly, and then sintered at high temperature in a reducing atmosphere to form a composite of antimony-tin alloy, water-soluble carbonate and carbon, and then washed with water to dissolve the carbonate formed in situ during the sintering process to obtain a multi-level porous structure, thereby obtaining a hierarchical porous carbon composite tin-antimony alloy material; The organic metal salt containing tin and alkali metal or the organic metal salt containing antimony and alkali metal is a compound composed of organic acid anion, tin cation or antimony cation, and alkali metal cation, part of which has crystal water, and the chemical general formula is C x H y O z A w B v uH2O, where A is Sn or Sb, B is an alkali metal, 0 <x,y,z<20,0<w,v<5,0≤u<10。 2. The preparation method according to claim 1, characterized in that: The organic acid anion is citrate, tartrate or gluconate, and the alkali metal cation is Na + or K + .
3. The preparation method according to any one of claims 1 to 2, characterized in that: The organic metal salt containing tin and alkali metal is disodium stannous citrate; the organic metal salt containing antimony and alkali metal is at least one of potassium antimony tartrate trihydrate, potassium antimony tartrate hemihydrate, sodium antimony L-tartrate and sodium antimony gluconate nonahydrate.
4. The preparation method according to claim 1, characterized in that: During the high-temperature sintering process in a reducing atmosphere, the organic ligands in the mixed organic metal salts are pyrolyzed to form a carbon skeleton, the alkali metal ions are converted into water-soluble carbonates as templates, the tin ions and antimony ions are reduced to elements and form tin-antimony alloy nanoparticles in situ, which are encapsulated in the carbon matrix to form a composite.
5. The preparation method according to claim 1, characterized in that The steps include: Step 1: Ball milling According to the Sn / Sb molar ratio of 1:1, an organic metal salt containing tin and an alkali metal and an organic metal salt containing antimony and an alkali metal are mixed and ball-milled at a ball-milling speed of 200-500 rpm for 2-6 h to obtain a precursor powder; Step 2: Reduction sintering The precursor powder is sintered at high temperature in a reducing atmosphere, with a gas flow rate of 20-100 sccm, a sintering temperature of 500-600°C, a sintering time of 1-3 h, a heating rate of 2-10°C / min, and a sintered powder is obtained after natural cooling; Step 3: Wash and remove the template: The sintered powder is soaked in deionized water for 1-6 hours, the soaking liquid is filtered out, and then washed with deionized water. After drying, a graded porous carbon composite tin-antimony alloy material is obtained.
6. The preparation method according to claim 1 or 5, characterized in that: The ball milling is dry ball milling without adding a dispersant or wet ball milling with adding an organic dispersant. After the dry ball milling, the precursor powder is directly obtained, and after the wet ball milling, the precursor powder is obtained by drying. The organic dispersant used in the wet ball milling is one of ethanol, acetone, and cyclohexane.
7. The preparation method according to claim 1 or 5, characterized in that: The reducing atmosphere is at least one of hydrogen, argon-hydrogen mixed gas, and nitrogen-hydrogen mixed gas.
8. A hierarchical porous carbon composite tin-antimony alloy material obtained by the preparation method according to any one of claims 1 to 7.
9. An alkali metal ion secondary battery, characterized in that: The negative electrode active material used includes the graded porous carbon composite tin-antimony alloy material as claimed in claim 8.