Method for additive manufacturing of gradient structure based on friction stir treatment technology

By combining friction stir processing and directional energy deposition in additive manufacturing, a gradient structure of fine grains and columnar crystals or equiaxed grains is formed, which solves the problems of lack of universality and time-consuming parameter debugging of gradient structure preparation in the existing technology. It achieves excellent mechanical properties and simplified process under different load-bearing conditions.

CN118720167APending Publication Date: 2024-10-01SHENYANG AEROSPACE UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410759063.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing additive manufacturing technology lacks universality when preparing gradient structures and is difficult to meet performance requirements under different loading conditions. Traditional process parameter debugging takes a long time and it is difficult to quickly achieve fine-grained gradient structures.

Method used

Friction stir treatment technology is combined with directional energy deposition to form a fine-grained structure through surface smoothing and friction stir treatment, control the depth of the shoulder deformation zone, combine mechanical processing and redeposition, and cycle until the preset height is reached to prepare a gradient tissue structure .

Benefits of technology

It achieves the distribution of fine grains and columnar grains or equiaxed grain gradient structures under different load-bearing conditions, improves the mechanical properties and service performance of the parts, simplifies the parameter debugging process, and improves the universality of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720167A_ABST
    Figure CN118720167A_ABST
Patent Text Reader

Abstract

The invention discloses a method for additive manufacturing of a gradient structure based on a stirring friction treatment technology, and belongs to the technical field of additive manufacturing. Through a directional energy deposition technology, after a fixed number of layers are deposited, the deposited layers are subjected to surface leveling treatment. Then, stirring friction treatment with a certain depth is carried out on the flat deposition layer, and a fine grain structure can be formed in a stirring area; and a shaft shoulder deformation area with a certain depth exists between the shaft shoulder in the stirring area and the tail area of the stirring needle. According to the prepared target gradient structure, the shaft shoulder deformation area is subjected to mechanical machining treatment, the shaft shoulder deformation area with a certain thickness is removed, meanwhile, the interlayer temperature is controlled to be 100 DEG C or below, deposition is conducted again, and the type of the target structure is determined by the remelting position. And when the height of the fixed deposition layer is reached again, after surface leveling is conducted, stirring friction treatment and deposition of a new layer are conducted again, circulation is conducted till the preset component height is obtained, and manufacturing of the gradient organization structure is completed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of additive manufacturing, and in particular relates to a method for additive manufacturing of gradient structures based on friction stir processing technology. Background Art

[0002] Additive Manufacturing (AM) technology uses heat sources to melt raw materials and deposit them layer by layer to obtain solid components. Due to its advantages such as rapid manufacturing, low material waste rate, no need for molds, and personalized customization, it has attracted much attention in the aerospace field in recent years. Directed energy deposition (DED) technology uses laser / arc as a heat source to melt metal powder or wire and send it into a molten pool for layer-by-layer deposition to complete the manufacture of metal structures. Due to the manufacturing characteristics of the molten pool's rapid melting and solidification, the layer-by-layer deposition process will undergo multiple thermal cycles, which can easily cause the metallurgical structure to transform into a coarse columnar crystal structure.

[0003] Taking titanium alloy forming as an example, there are epitaxially grown coarse columnar crystals in the metallurgical structure formed by directed energy deposition, and only a small amount of equiaxed crystals or fine grains exist at the bottom and top, resulting in anisotropy of part performance. Nevertheless, epitaxially grown coarse columnar crystals also have some advantages. When the component is loaded in a direction perpendicular to the substrate, the columnar crystals of the fiber structure have a certain positive effect on the improvement of strength; on the contrary, when loaded in the horizontal direction, the performance will be greatly reduced, which seriously affects the service performance of the parts. At the same time, according to the Hall-Petch theoretical formula, the finer the grains and the more grain boundaries inside the metal material, the greater the resistance to dislocation movement, and the cracks are not easy to initiate and expand, which makes the material have good fracture toughness. Severe plastic deformation (SPD) achieves improvement and refinement of the organization through severe plastic deformation. It is the most potential method to achieve organizational improvement and the most effective method.

[0004] Friction stir processing (FSP) is a processing method evolved from friction stir welding. The strong stirring action of friction stir processing can cause the processed materials to undergo severe plastic deformation, mixing, and crushing, achieving the densification, homogenization, and refinement of the microstructure, thereby improving the material properties. Therefore, friction stir processing can achieve the improvement and refinement of additive manufacturing organization, and can complete the design of gradient organization through coordination with mechanical processing.

[0005] CN112170837A discloses a method for laser additive manufacturing of titanium alloys with gradient organizational characteristics. The preparation process is to control the scanning speed between different overlap passes and a specific scanning path, with a higher scanning speed for the outer layer and a lower scanning speed for the inner layer. Finally, a gradient organizational structure with fine β columnar crystals in the outer layer and coarse columnar crystals in the innermost layer is obtained by layer-by-layer deposition. However, this method is not universal. The invention only prepares gradient organizations by adjusting parameters, which is obviously not applicable to the preparation of gradient organizations by additive manufacturing technologies with other heat source types.

[0006] CN111299583A discloses a method for laser additive manufacturing of gradient structure titanium alloy integral components. Based on the optimized process parameters, the process is to match the powder feeding amount with the equiaxed crystal volume fraction in the single-pass deposition layer, and control the remelting depth at the same time. Finally, the relationship between the remelting depth and width and the equiaxed crystal volume fraction is established, and the "columnar crystal-equiaxed crystal-columnar crystal" gradient structure is obtained, which can achieve the organizational characteristics of different parts of the overall parts. The method establishes a method for preparing gradient structures by coupling parameters with remelting depth. However, there are many parameter variables in the additive manufacturing process, and it takes a long time to debug and optimize the parameters if the implementation of the solution is to be completed quickly.

[0007] In summary, the common means of preparing gradient structures in the additive manufacturing process is to adjust or optimize the process parameters, and the preparation method of gradient structures is not universal. At the same time, for some situations with high load intensity, it is difficult for the traditional process to prepare gradient structures to meet the service conditions. Therefore, it is very necessary to develop a fine-grained gradient structure with good universality and applicable to different load conditions to realize the overall part structure design. Summary of the invention

[0008] The object of the present invention is to provide a method for collaboratively preparing gradient structures suitable for different load conditions by friction stir processing and additive manufacturing.

[0009] Through the directed energy deposition technology, after depositing a fixed number of layers, the deposited layer is surface-leveled. Subsequently, a stir friction treatment of a certain depth is performed on the flat deposited layer, and a fine-grained structure will be formed in the stirring zone; there is a shoulder deformation zone of a certain depth in the shoulder and the tail area of ​​the stirring needle in the stirring zone. According to the prepared target gradient structure, the shoulder deformation zone is mechanically processed to remove a certain thickness of the shoulder deformation zone, and the interlayer temperature is controlled to be below 100°C for re-deposition. The remelting position determines the target structure type. When the fixed deposition layer height is reached again, after surface leveling, stir friction treatment and deposition of a new layer are performed again, and the cycle is repeated until the preset component height is obtained, that is, the manufacture of the gradient structure is completed.

[0010] To achieve the above object, the present invention adopts the following technical solutions:

[0011] A method for additively manufacturing a gradient structure based on a friction stir processing technique comprises the following steps:

[0012] (1) According to the 3D digital model of the part, layered slicing is performed, and the corresponding forming trajectory is divided to output the program code, and the program code is imported into the corresponding forming motion actuator, namely, the additive manufacturing system, the mechanical processing system and the stir friction processing system; wherein the layered slicing thickness is less than 2 mm;

[0013] (2) drying the wire or powder, cleaning the substrate surface with acetone after removing the oxide layer, and fixing the substrate on a workbench;

[0014] (3) Melting the corresponding wire or powder and depositing it layer by layer to form a deposition layer; wherein the thickness of the deposition layer is less than 1.2 times the length of the stirring needle, and the specific number of layers is selected according to the thickness of the single layer of different additive manufacturing and the stirring needle;

[0015] (4) using mechanical processing equipment to smooth the surface of the deposited layer;

[0016] (5) Drill a hole at one end of the flat surface of the sedimentary layer. The hole depth is equal to the length of the stirring needle (the stirring needle length is less than 10 mm), and the hole diameter is slightly smaller than the diameter of the tail of the conical stirring needle. The difference is 0.5 to 1 mm.

[0017] (6) inserting a stirring head into the blind hole to perform friction stirring treatment on the deposited layer, thereby forming a fine-grained stirring zone;

[0018] (7) Control the thickness of the deposited layer removed by mechanical processing, and deposit again to achieve the preparation of different structural gradient organizations;

[0019] (8) Based on the part manufactured by the composite process, the residence time (120s to 180s) is controlled to ensure that the upper surface temperature of the sample after machining is below 100°C, and steps (4) to (7) are repeated alternately until the fine-grained-gradient microstructure is completed as a whole.

[0020] The method can be applied to the preparation of thin-wall gradient structures, surface layer gradient tissue structures and space grid gradient tissue structures;

[0021] In step (3), the deposition heat source used in the melting process is one of a laser, an arc, an electron beam, and an ion beam;

[0022] During the additive deposition process, the height of the deposited layer is

[0023] n*Δh<1.2H

[0024] Where n is the number of layers, Δh is the layer thickness, and H is the depth of the stirring zone;

[0025] In step (4), during the surface smoothing process, the thickness of the material removed is 0.2H; H is consistent with the length of the stirring needle and is limited by the physical properties of different materials and is less than 10mm;

[0026] In step (6), during the friction stir treatment, the depth of the shoulder deformation zone generated is H S =H m +H Re ; Among them, H S is the depth of the shoulder deformation zone (the deformation depth near the shoulder in the stirring zone), H m is the thickness of the deposited layer removed by machining, H Re is the remaining depth of the shoulder deformation zone; where H S is the depth of the shoulder deformation zone (the deformation depth near the shoulder in the stirring zone), H m is the thickness of the deposited layer removed by machining, H Re It is the remaining depth of the shoulder deformation zone.

[0027] In step (7), the structure type of the newly deposited layer is determined by the remelting depth H R and the remaining depth H of the shoulder deformation zone Re The criteria for determining whether the shoulder deformation zone is retained are:

[0028] (1)H Re <H R , the entire shoulder deformation zone is remelted, and epitaxial growth continues in the upper area of ​​the original columnar crystal structure, forming a gradient structure with fine crystals in the middle and columnar crystals on both sides;

[0029] (2)H Re >H R , partial remelting occurs in the shoulder deformation zone, and the new deposition layer nucleates and grows in the fine-grained area. The middle area is still fine-grained, and a gradient structure of equiaxed crystals is formed on both sides.

[0030] Control the remaining depth H of the shoulder deformation zone Re The processing means is one of milling and grinding, and the processing equipment is one of milling machine, grinder, and robotic arm-electric spindle.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) In the process of directed energy deposition additive manufacturing, the present invention introduces interlayer stirring treatment to cause severe plastic deformation of the deposited layer. While the grains are refined, defects such as pores and microcracks inside the deposited layer are also eliminated, thereby improving the internal quality of the component.

[0033] (2) In the process of directed energy deposition additive manufacturing, the present invention introduces interlayer stirring treatment to cause severe plastic deformation of the deposited layer, and ultimately obtains a gradient microstructure with a fine-grained area in the middle and either columnar crystal areas or equiaxed crystal areas on both sides.

[0034] (3) In the process of directed energy deposition additive manufacturing, the present invention performs interlayer stirring treatment on the deposited layer, and realizes the gradient distribution of columnar crystal structure (or equiaxed crystal structure) and fine crystal at any position of the structural part by adjusting relevant parameters and the moving trajectory of the stirring treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of preparing different types of gradient tissues under composite manufacturing process;

[0036] Figure 2 Flow chart of composite manufacturing process for preparing gradient tissue;

[0037] Figure 3 Schematic diagram of the composite additive manufacturing process;

[0038] Figure 4 Schematic diagram of the processing dimensions of the composite manufacturing process; where (a) is a deposition layer with n layers, (b) is a deposition layer after mechanical processing, (c) is a deposition layer after stirring, (d) is a stirring zone after mechanical processing, and (e) is a deposition layer after additive manufacturing.

[0039] Figure 5 Gradient organizational structure; wherein, (a) is the surface layer gradient organizational structure, (b) is the space grid gradient organizational structure;

[0040] Among them, 1-thin wall structure, 2-substrate, 3-fine crystal area, 4-columnar crystal area, 5-equiaxed crystal area, 6-additive deposition equipment, 7-machining equipment, 8-friction stir equipment. DETAILED DESCRIPTION

[0041] The present invention generates fine-grained structure in the structure manufactured by directed energy deposition through the stir friction processing technology, and then obtains the stirring zone and the shoulder deformation zone above it. Through subsequent interlayer machining, the depth of the shoulder deformation zone is controlled according to the need to prepare equiaxed crystals or columnar crystal structures. When the shoulder deformation zone is less or does not exist, the previous deposition layer will be completely remelted, and the newly formed structure will continue to grow epitaxially on the basis of the original structure, and finally form a gradient structure with fine crystals in the middle and columnar crystals on both sides of the wall; when the shoulder deformation zone is retained more, the remelting depth is not enough to make all the shoulder deformation zones remelt, and at this time there are more nucleation sites on the basis of the original shoulder deformation zone structure, so the newly formed structure on both sides of the wall exists in the form of equiaxed crystal structure. Finally, a gradient structure with fine crystals in the middle and equiaxed crystals on both sides is formed.

[0042] The gradient structure prepared by this method is an alternating structure of fine crystals and columnar crystals or equiaxed crystals. The gradient structure prepared by this method is shown in the figure of a thin wall. Figure 1 As shown in the figure, structure I is a structure with fine crystals in the middle and columnar crystals on both sides, which has strong vertical bearing capacity; structure II is a structure with fine crystals in the middle and equiaxed crystals on both sides, which has strong horizontal bearing capacity. Therefore, the two gradient organizations have excellent mechanical properties under different load conditions and can show good service performance. Among them, the composite manufacturing process for preparing gradient organizations is as follows Figure 2 shown.

[0043] Example 1

[0044] The steps of the method for additive manufacturing of gradient structure organization based on friction stir processing technology in this embodiment are as follows:

[0045] (1) The digital model of the part with a size of 100 mm × 20 mm × 50 mm is sliced ​​and divided into corresponding forming trajectories and program codes are generated using professional slicing software.

[0046] (2) After the preliminary process parameter optimization, the arc additive manufacturing process parameters are: pulse current is 150A-110A, travel speed is 2mm / s, wire feeding rate is 1.5m / min, and argon as a shielding gas flow rate is 15L / min.

[0047] (3) After drying the raw materials of the wire, Figure 3 As shown, the deposition device 6 follows the generated program to perform multi-pass multi-layer deposition of TC4 titanium alloy. The number of deposition layers is n = 2 layers, and the thickness Δh = 1.5 mm. Each layer is overlapped for six times, and the overlap rate is 50%, and finally a deposition layer with a height of n*Δh = 3 mm is obtained, as shown in FIG. Figure 4 (a) shown.

[0048] (4) Figure 3 As shown, the upper surface of the deposited layer is then flattened using a machining device 7, and the thickness of the deposited layer removed is about 0.2H = 0.5 mm. Figure 4 (b) as shown.

[0049] (5) Figure 3 As shown, the friction stir treatment device 8 moves along the long side of the specimen to perform friction stir treatment on the deposited layer. The stirring needle is conical, with a diameter of 4 mm and 6 mm from the tip to the tail, a shoulder diameter of 15 mm, and a needle length H = 2.5 mm. During the friction stir treatment, the stirring head speed is 250 rpm, the travel speed is 50 mm / min, and after treatment, the following is obtained in the middle of the specimen: Figure 4 (c) shows the stirring zone (including the shoulder deformation zone and the weld core zone). The depth of the shoulder deformation zone H SThe remelting depth H of this parameter arc additive is 1.25mm. R It is 0.25mm.

[0050] (6) Machining treatment is performed on the surface of the deposited layer, such as Figure 4 As shown, the machining device 9 removes the thickness H m Materials such as Figure 4 (d). By controlling H m The processing depth is such that when remelting occurs, the structures on both sides will be in different forms. Figure 4 (e) The position shown is formed. m =1.1mm, H Re <H R , that is, the deposited layer remelts, and the original columnar crystal structure on both sides continues to grow epitaxially. When Hm = 0.5 mm, H Re >H R , the structure undergoes nucleation and growth in the recrystallization zone, and grows in the form of equiaxed crystals on both sides.

[0051] (7) After a certain period of interlayer dwelling, arc additive deposition is continued until the height reaches (n-1)*Δh=1.5 mm, and operations (4) to (6) are repeated until the target height of the model is obtained. Finally, different gradient microstructures of arc additive composite stirring treatment are obtained. The gradient microstructure is as follows: Figure 5 shown.

[0052] Example 2

[0053] The steps of the method for additive manufacturing of gradient structure organization based on friction stir processing technology in this embodiment are as follows:

[0054] (1) The digital model of the part with a size of 100 mm × 20 mm × 50 mm is sliced ​​and divided into corresponding forming trajectories and program codes are generated using professional slicing software.

[0055] (2) After the preliminary process parameter optimization, the laser additive manufacturing process parameters are: laser power = 1800 W, scanning speed = 0.6 m / min, powder feeding rate = 15 g / min, overlap rate = 50%, and a flexible argon protective cover is used as a protective device.

[0056] (3) After drying the powder raw materials, Figure 3 As shown, the deposition device 6 follows the generated program to perform serpentine reciprocating scanning along the short side. The number of deposition layers is n = 4 layers, and the thickness Δh = 0.8 mm. Finally, a deposition layer with a height of n*Δh = 3.2 mm is obtained, as shown in FIG. Figure 4 (a) shown.

[0057] (4) Figure 3As shown, the upper surface of the deposited layer is then flattened using a machining device 7, and the thickness of the deposited layer removed is about 0.2H = 0.54 mm. Figure 4 (b) as shown.

[0058] (5) Figure 3 As shown, the friction stir treatment device 8 moves along the long side of the specimen to perform friction stir treatment on the deposited layer. The stirring needle is conical, with a diameter of 4 mm and 6 mm from the tip to the tail, a shoulder diameter of 15 mm, and a needle length H = 2.7 mm. During the friction stir treatment, the stirring head speed is 250 rpm, the travel speed is 50 mm / min, and after treatment, the following is obtained in the middle of the specimen: Figure 4 (c) shows the stirring zone (including the shoulder deformation zone and the weld core zone). The depth of the shoulder deformation zone H S The remelting depth H of laser additive under this parameter is 1.25 mm. R It is 0.2mm.

[0059] (6) Machining treatment is performed on the surface of the deposited layer, such as Figure 4 As shown, the machining device 9 removes the thickness H m Materials such as Figure 4 (d). By controlling H m The processing depth is such that when remelting occurs, the structures on both sides will be in different forms. Figure 4 (e) The position shown is formed. m =1.1mm, H Re <H R , that is, the deposited layer remelts, and the original columnar crystal structure on both sides continues to grow epitaxially. m =0.5mm, H Re >H R , the structure undergoes nucleation and growth in the recrystallization zone, and grows in the form of equiaxed crystals on both sides.

[0060] (7) After a certain period of interlayer dwelling, laser additive deposition is continued to reach a height of (n-1)*Δh=2.4 mm, and operations (4) to (6) are repeated until the target height of the model is obtained, and finally different gradient microstructures of laser additive composite stirring treatment are obtained.

Claims

1. A method for additive manufacturing of gradient structures based on friction stir processing technology, It is characterized in that The following steps are involved: (1) According to the 3D digital model of the part, the part is sliced ​​and divided into corresponding forming trajectories to output program codes, and the program codes are imported into the corresponding actuators of the forming motion, namely, the additive manufacturing system, the machining system, and the friction stir processing system; (2) drying the wire or powder, removing the oxide layer from the substrate, cleaning the substrate surface, and fixing it on a workbench; (3) melting the corresponding wire or powder and depositing layer by layer to form a deposition layer; (4) using mechanical processing equipment to smooth the surface of the deposited layer; (5) Drill a hole at one end of the flat surface sediment layer, the hole depth is equal to the length of the stirring needle, and the hole diameter is smaller than the diameter of the tail of the conical stirring needle, and the difference is 0.5 to 1 mm; (6) inserting a stirring head into the blind hole to perform friction stirring treatment on the deposited layer, thereby forming a fine-grained stirring zone; (7) Control the thickness of the deposited layer removed by mechanical processing, and deposit again to achieve the preparation of different structural gradient organizations; (8) Based on the part manufactured by the composite process, the residence time is controlled to be 120 s to 180 s to ensure that the upper surface temperature of the sample after machining is below 100° C. Steps (4) to (7) are repeated alternately until the fine-grained-gradient microstructure is completed as a whole.

2. A method for additive manufacturing of gradient structures based on friction stir processing technology according to claim 1, It is characterized in that The method can be applied to the preparation of thin-wall gradient structures, surface layer gradient tissue structures and space grid gradient tissue structures.

3. A method for additive manufacturing of gradient structures based on friction stir processing technology according to claim 1, It is characterized in that In step (1), the thickness of the layered slices is less than 2 mm.

4. The method for additive manufacturing of gradient structures based on friction stir processing technology according to claim 1, It is characterized in that In step (2), acetone is used to clean the surface of the substrate.

5. The method for additive manufacturing of gradient structures based on friction stir processing technology according to claim 1, It is characterized in that In step (3), the deposition heat source used in the melting process is one of a laser, an arc, an electron beam, and an ion beam; The thickness of the deposited layer is less than 1.2 times the length of the stirring needle. The specific number of layers depends on the thickness of the single layer of additive manufacturing and the selection of the stirring needle.

6. The method for additive manufacturing of gradient structures based on friction stir processing technology according to claim 1, It is characterized in that In step (3), during the additive deposition process, the height of the deposited layer is n*Δh<1.2H Where n is the number of layers, Δh is the layer thickness, and H is the depth of the stirring zone.

7. A method for additively manufacturing gradient structures based on friction stir processing technology according to claim 1 or 6, It is characterized in that In step (4), during the surface smoothing process, the thickness of the material removed is 0.2H; H is consistent with the length of the stirring needle and is limited by the physical properties of different materials and has a value of <10 mm.

8. The method for additive manufacturing of gradient structures based on friction stir processing technology according to claim 1, It is characterized in that In step (6), during the friction stir treatment, the depth of the shoulder deformation zone generated is H S =H m +H Re ; Among them, H S is the depth of the shoulder deformation zone (the deformation depth near the shoulder in the stirring zone), H m is the thickness of the deposited layer removed by machining, H Re is the remaining depth of the shoulder deformation zone; where H S is the depth of the shoulder deformation zone (the deformation depth near the shoulder in the stirring zone), H m is the thickness of the deposited layer removed by machining, H Re It is the remaining depth of the shoulder deformation zone.

9. The method for additive manufacturing of gradient structures based on friction stir processing technology according to claim 1, It is characterized in that In step (7), the structure type of the newly deposited layer is determined by the remelting depth H R and the remaining depth H of the shoulder deformation zone Re The criteria for determining whether the shoulder deformation zone is retained are: (1)H Re <H R , the entire shoulder deformation zone is remelted, and epitaxial growth continues in the upper area of ​​the original columnar crystal structure, forming a gradient structure with fine crystals in the middle and columnar crystals on both sides; (2)H Re >H R , partial remelting occurs in the shoulder deformation zone, and the new deposition layer nucleates and grows in the fine-grained area. The middle area is still fine-grained, and a gradient structure of equiaxed crystals is formed on both sides.

10. A method for additive manufacturing of gradient structures based on friction stir processing technology according to claim 9, It is characterized in that Control the remaining depth H of the shoulder deformation zone Re The processing means is one of milling and grinding, and the processing equipment is one of milling machine, grinder, and robot arm-electric spindle.