Visual semi-permanent mold release agent as well as preparation method and application thereof

Through the polymerization reaction of vinyl-terminated siloxane compounds and tetrazine compounds, combined with amino silicone oil and solvents, a high-temperature-resistant and wear-resistant release agent is prepared, which solves the problem of existing release agents at high temperatures. Solve the problem of insufficient performance and achieve more efficient demoulding times and production efficiency.

CN118721540AActive Publication Date: 2024-10-01SHANGHAI UNIV OF ENG SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411006139.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-01
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Existing release agents are not durable at high temperatures, and their mechanical wear and impact resistance are insufficient, resulting in limited demoulding times and affecting production efficiency.

Method used

Use vinyl-terminated siloxane compounds and tetrazine compounds to polymerize at 0-80°C, and add amino silicone oil and solvent to form a release agent with high cross-linking density and indicator color to improve its rigidity and heat resistance. stability.

Benefits of technology

It improves the high temperature resistance, wear resistance and impact resistance of the release agent, increases the number of demoulding times, improves production efficiency, and facilitates timely replacement through color indication to ensure product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721540A_ABST
    Figure CN118721540A_ABST
Patent Text Reader

Abstract

The invention discloses a visual semi-permanent mold release agent as well as a preparation method and application thereof, and belongs to the technical field of mold release agents. The release agent comprises the following raw material components: a vinyl-terminated siloxane compound, a tetrazine compound, amino silicon oil and a solvent in a mass volume ratio of 1g: (0.05-0.15) g: (0.01-0.05) g: (10-100) mL. According to the prepared mold release agent, due to the addition of the tetrazine compound, the cross-linking density between molecules of the tetrazine compound and the vinyl-terminated siloxane compound is increased, the rigidity of the mold release agent is improved, or the strength of the mold release agent is adjusted by changing the acting force between the molecules, so that the mold release agent has a certain rigid mechanical property; the wear resistance and the impact resistance are enhanced, so that the demolding frequency is increased, and the production efficiency is improved; the heat stability is improved, the high temperature resistance is realized, and the application range is wider.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a visual semi-permanent demoulding agent and a preparation method and application thereof, belonging to the technical field of demoulding agents, and is suitable for an external demoulding system, in particular for an external demoulding system for producing plastic products. Background Art

[0002] A release agent is a functional substance between the mold and the finished product. During the molding process, physical or chemical adsorption will form between the product and the mold, making it difficult to remove the molded product from the mold. The use of a release agent can smoothly separate the solidified product from the mold, thereby obtaining a smooth and flat product and ensuring that the mold can be used multiple times.

[0003] Generally speaking, the mold release agents currently used in plastic products are mainly silicone mold release agents, which are widely used in various occasions such as plastics and rubber due to their low surface tension, good leveling, high temperature resistance, non-toxicity, good gloss, and no affinity with resin. In order to improve the mechanical friction resistance of silicone mold release agents, the mold release agent components need to be modified.

[0004] US20180346661 discloses an organosiloxane emulsion composition, and finds that an organosilicone emulsion composition containing a high-viscosity organopolysiloxane and an organosiloxysilicate containing a polyether group is mixed with an organopolysiloxane having polyoxyalkylene residues at both ends, and an emulsion with good stability in a water-soluble solvent is successfully obtained. This release agent is modified to improve its demoulding properties and emulsion stability, but this release agent is easily transferred from the mold to the product, and it is impossible to achieve multiple demoulding after applying it once. Therefore, the release agent needs to be frequently applied to the mold, which ultimately affects production efficiency.

[0005] US4244912A discloses a curable siloxane composition, which is composed of polydiorganosiloxane, xylene soluble copolymer, methyl hydrogen polysiloxane and hydrosilylation catalyst. The composition can be quickly cured at low temperature and is wear-resistant, and can be used as a curable release agent, especially in a molding method using a "cold molding" polyurethane composition. Although the curable release agent can achieve multiple demolding and the amount of the release agent transferred from the mold to the product is small, the release agent is not resistant to high temperatures, which limits the scope of application of the release agent.

[0006] CN1671794A discloses a curable composition with demoulding properties, which comprises an ethylene polymer containing an alkenyl group, a compound containing a hydrosilyl group, a hydrosilylation catalyst, and a metal soap. The curable composition has good mechanical properties, oil resistance, heat resistance, demoulding properties, etc., but the thermal curing temperature of the composition needs to be above 100°C, resulting in energy waste and complicated operation.

[0007] Therefore, if a release agent with fast film-forming, high temperature resistance, wear resistance and impact resistance can be prepared, it will be of great significance in the field of release agents and have broad market prospects. Summary of the invention

[0008] The invention provides a visual semi-permanent release agent and a preparation method and application thereof, aiming to prepare a release agent with rapid film formation, high temperature resistance, wear resistance and impact resistance, increase the number of demoulding times and improve production efficiency.

[0009] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:

[0010] A visual semi-permanent release agent, the general structural formula of the release agent is as follows:

[0011]

[0012] Wherein: the R1-R8 are independent of each other, and R1-R8 are selected from the following identical or different straight-chain or branched alkyl, alkenyl, cycloalkyl or cycloalkenyl, aryl or aromatic hydrocarbon groups, n is an integer of 1-30, and the sum of x+y is an integer of 1-1000.

[0013] Preferably, R1-R8 are selected from C1-C6 alkyl or alkenyl groups.

[0014] Preferably, the structural formula of the release agent is as follows:

[0015]

[0016] Wherein, x+y=an integer of 300-500, and n is an integer of 2-5.

[0017] A method for preparing a visual semi-permanent release agent, the reaction process of which is as follows:

[0018]

[0019] The polysiloxane is prepared by polymerization of a vinyl-terminated siloxane compound and a tetrazine compound at 0-80°C, preferably at 60°C.

[0020] Preferably, the polymerization reaction is performed by stirring, cooling and standing the vinyl-terminated siloxane compound and the tetrazine compound.

[0021] Furthermore, the stirring speed is 100-2000 rpm, and the stirring time is 3-15 h.

[0022] Furthermore, the stirring speed is 1000 rpm and the stirring time is 10 h.

[0023] Preferably, in the tetrazine compound, n is an integer of 1-30.

[0024] Furthermore, n is 2-30.

[0025] Furthermore, n is 2-5.

[0026] Preferably, the general structural formula of the vinyl-terminated siloxane compound is as follows:

[0027]

[0028] Furthermore, the general structural formula of the vinyl-terminated siloxane compound is as follows:

[0029] ViMe2SiO(Me2SiO) x SiMe2Vi, then y = 0; or,

[0030] ViPhMeSiO(Me2SiO) x SiMePhVi, then y = 0; or,

[0031] ViMe2SiO(Me2SiO) x (ViMeSiO) y SiMe2Vi; or,

[0032] ViPhMeSiO(Me2SiO) x (ViMeSiO) y SiMePhVi;

[0033] Wherein: Me, Et, Ph and Vi represent methyl, ethyl, phenyl and vinyl respectively, and the sum of x+y is an integer of 1-1000.

[0034] Furthermore, the vinyl-terminated siloxane compound has the following two structural formulas:

[0035] ViMe2SiO(Me2SiO) x (ViMeSiO) y SiMe2Vi, wherein the sum of x+y is an integer from 300 to 500; or, ViMe2SiO(Me2SiO) x SiMe2Vi, wherein x is an integer from 300 to 500.

[0036] The preparation method of the mold release agent composition comprises the following steps: stirring a vinyl-terminated siloxane compound, a tetrazine compound, an amino silicone oil and a solvent in a mass volume ratio of 1 g: 0.05-0.15 g: 0.01-0.05 g: 10-100 mL to obtain the mold release agent composition.

[0037] Preferably, in the method for preparing the release agent composition, the mass volume ratio of the vinyl-terminated siloxane compound, the tetrazine compound, the amino silicone oil and the solvent is 1 g: 0.1 g: 0.02 g: 100 mL, and the molecular weight of the amino silicone oil is 1000-100000.

[0038] Furthermore, the solvent is one or more of alcohol solvents, alcohol ether solvents, ketone solvents, ester solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents and ether solvents.

[0039] Furthermore, the alcohol solvent is one or more of ethanol, isopropanol, propylene glycol, butanol, 1,4-butanediol, 1,3-butanediol and glycerol;

[0040] The alcohol ether solvent is one or more of ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monobutyl ether;

[0041] The ketone solvent is one or more of acetone, butanone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone;

[0042] The ester solvent is one or more of methyl acetate, ethyl acetate and butyl acetate;

[0043] The aliphatic hydrocarbon solvent is one or more of n-hexane, carbon tetrachloride, petroleum ether, and isoparaffin (C8-C10);

[0044] The alicyclic hydrocarbon solvent is one or both of cyclopentane and cyclohexane;

[0045] The aromatic hydrocarbon solvent is one or both of toluene and xylene;

[0046] The ether solvent is one or more of tetrahydrofuran, diisopropyl ether and dibutyl ether.

[0047] Preferably, during the preparation of the release agent composition, the stirring speed is 100-2000 rpm, and the stirring time is 1-5 h.

[0048] Furthermore, during the preparation of the release agent composition, the stirring speed was 1000 rpm and the stirring time was 3 h.

[0049] Application of the above-mentioned visual semi-permanent release agent or the above-mentioned release agent composition in the preparation of external release system products.

[0050] Preferably, the external mold release system products are plastic products and rubber products of the external mold release system.

[0051] Furthermore, the plastic products include polyurethane foam products, epoxy resin products, glass fiber reinforced epoxy resin products, and unsaturated polyester products.

[0052] The beneficial effects of the present invention are:

[0053] (1) Due to the addition of tetrazine compounds, the mold release agent or mold release agent composition prepared by the present invention improves the rigidity of the mold release agent by increasing the crosslinking density between the tetrazine compound and the vinyl-terminated siloxane compound molecules, or adjusts its strength by changing the intermolecular force, so that the mold release agent has certain rigid mechanical properties, enhances the wear resistance and impact resistance, thereby increasing the number of demolding times and improving production efficiency;

[0054] (2) Through testing, it is found that the addition of tetrazine compounds improves the thermal stability of the release agent, making the release agent resistant to high temperatures and having a wider range of applications;

[0055] (3) In addition, the tetrazine compound is a purple solid, and the color becomes lighter to light purple after the reaction with the vinyl-terminated siloxane compound is complete; the addition of the tetrazine compound has an indicator effect on the preparation of the release agent, and also has an indicator effect during the use of the release agent. When the color disappears, it needs to be reapplied;

[0056] (4) The release agent or release agent composition of the present invention has the characteristics of simple composition, rapid curing, extremely low transfer rate, good storage stability, high temperature resistance, and indicator function. In addition, the isolation film has certain mechanical properties, which improves the wear resistance and impact resistance, thereby ensuring smooth production while improving production efficiency and reducing product defects. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 The figures are the film formation of release agent compositions 1-6 on the mold surface in Test 2, wherein (a) is release agent composition 1, (b) is release agent composition 2, (c) is release agent composition 3, (d) is release agent composition 4, (e) is release agent composition 5, and (f) is release agent composition 6;

[0058] Figure 2 This is a TGA graph of thermal stability of the release agent composition in Test 4, wherein the abscissa is temperature (° C.) and the ordinate is weight percentage (%). DETAILED DESCRIPTION

[0059] In order to make the technical means, creative features, objectives and effects of the present invention easier to understand, the present invention is further described below with reference to specific illustrations.

[0060] The most commonly used release agent or release agent composition on the market is an external release agent, which is directly applied to the mold surface when used. After standing for a period of time, a smooth and dense isolation film is formed on the mold surface, thereby separating the mold from the processed material. The external release agent must be able to combine well with the mold surface, adhere to the mold surface more firmly without transferring to the product, but have no reaction or adhesion with the product. In addition, since there is a certain impact force when the mold is injected with raw materials, the isolation film formed by the release agent on the mold surface is preferably with certain rigid mechanical properties, impact resistance, and wear resistance.

[0061] In the present invention, "semi-permanent mold release agent" means that the main component of the mold release agent forms a cross-linkable polymer in an inert solvent, which is coated on the mold surface through a solution, and a complete and uniform isolation film is formed on the entire mold surface after the solvent evaporates and the solute solidifies; this isolation film has a certain rigid mechanical strength and can effectively resist the damage of the shear force generated during the demolding process, so that 15-25 demoldings can be achieved after one coating.

[0062] “Visualization” means that the release agent in the present invention has a light purple color, which serves as an indicator during the preparation and use of the release agent. When most of the color disappears, it needs to be reapplied.

[0063] It should be noted that the following substances in some embodiments of the present invention are obtained by purchasing commercially available products, as shown in Table 1.

[0064] Table 1:

[0065]

[0066]

[0067] The molds used in the following embodiments of the present invention are molds made of the following materials:

[0068] The release agent of the present invention can be applied to the molding mold by any suitable method, such as by spraying, brushing or rolling. The mold can be a metal material, such as aluminum, nickel, stainless steel, brass, etc., or a non-metallic material, such as a resin material, etc.

[0069] Example 1 Preparation of Tetrazine Compound 1

[0070] Sulfur (0.64 g, 10 mmol) was added to a terephthalonitrile (1.28 g, 10 mmol) aqueous solution (7 mL), and hydrazine hydrate (10 mL, 164 mmol) was added to the solution heated under reflux at 100°C for 8 hours. The resulting yellow precipitate was washed with cold ethanol (3×10 mL) and allowed to stand in air for 3 hours to obtain a purple solid (1.32 g, 20%), which was tetrazine compound 1, and its structural formula is as follows:

[0071] n is an integer from 2 to 5.

[0072] Wherein: The mass spectrum of tetrazine compound 1 is as follows:

[0073] 546.18(100.0%),547.18(32.7%),548.18(6.5%),547.17(4.4%).

[0074] Example 2 Preparation of Tetrazine Compound 2

[0075] This example is basically the same as Example 1, except that, in this example, hydrazine hydrate (10 mL, 164 mmol) was refluxed in a 100° C. solution for 15 h; a purple solid (2.87 g, 23%) was obtained, which is tetrazine compound 2, and its structural formula is as follows:

[0076] n is an integer from 6 to 30.

[0077] Wherein: The mass spectrum of tetrazine compound 2 is as follows:

[0078] 1326.40(100.0%),1327.40(76.1%),1328.40(37.3%),1327.39(11.8%),1329.41(7.0%),1329.40(3.4%),1330.41(1.3%),1330.40(1.0%).

[0079] Example 3 Preparation of Release Agent Composition 1

[0080] The chemical reaction process is as follows:

[0081]

[0082] That is, 5 g of Polymer VS 500, 0.5 g of 3,6-diphenyl-1,2,4,5-tetrazine, 10 mL of ethanol, and 90 mL of isodecane were added into a reactor respectively, stirred for 10 hours at 60° C. and 1000 rpm for the first time, and allowed to cool to room temperature. Then, 0.01 g of aminosilicone oil was added into the reactor, stirred for 3 hours at room temperature and 1000 rpm for the second time, and allowed to stand to obtain a release agent composition 1.

[0083] Example 4 Preparation of Release Agent Composition 2

[0084] The chemical reaction process is as follows:

[0085]

[0086] This embodiment is substantially the same as the embodiment 3, except that, in this embodiment, the 3,6-diphenyl-1,2,4,5-tetrazine in the embodiment 3 is replaced with the tetrazine compound 1 prepared in the embodiment 1, so as to prepare the release agent composition 2.

[0087] Example 5 Preparation of Release Agent Composition 3

[0088] The chemical reaction process is as follows:

[0089]

[0090] This embodiment is substantially the same as the embodiment 3, except that, in this embodiment, the 3,6-diphenyl-1,2,4,5-tetrazine in the embodiment 3 is replaced with the tetrazine compound 2 prepared in the embodiment 2, so as to prepare the release agent composition 3.

[0091] Example 6 Preparation of Release Agent Composition 4

[0092] The chemical reaction process is as follows:

[0093]

[0094] This embodiment is substantially the same as embodiment 3, except that Polymer VS 500 is replaced with Polymer RV5000 to prepare a release agent composition 4.

[0095] Example 7 Preparation of Release Agent Composition 5

[0096] The chemical reaction process is as follows:

[0097]

[0098] This embodiment is substantially the same as embodiment 4, except that Polymer VS 500 is replaced with Polymer RV5000 to prepare a release agent composition 5.

[0099] Example 8 Preparation of Release Agent Composition 6

[0100] The chemical reaction process is as follows:

[0101]

[0102] This embodiment is substantially the same as embodiment 5, except that Polymer VS 500 is replaced with Polymer RV5000 to prepare a release agent composition 6.

[0103] The following tests were performed on the release agent compositions 1-6 prepared in Examples 3-8:

[0104] Test 1 Stability test of release agent compositions 1-6

[0105] The release agent compositions 1-6 prepared in Examples 3-8 were mixed with 191 unsaturated resin respectively and heated at 100° C. for 24 hours. Compared with the 191 unsaturated resin without the release agent compositions 1-6, it can be seen that the release agent compositions 1-6 did not react with the 191 unsaturated resin.

[0106] Test 2 Storage stability test of release agent compositions 1-6

[0107] The release agent compositions 1-6 prepared in Examples 3-8 were left to stand at (30±2)° C., and it was found that the release agent compositions 1-6 could all be stably present for 12 months.

[0108] Test 3 Film-forming property test of release agent compositions 1-6

[0109] Take the release agent compositions 1-6 prepared in Examples 3-8, and use a cotton ball to evenly apply the release agent compositions 1-6 on the cleaned and dried molds in a circle method, and the application thickness is 0.05-5 μm, and 0.1-2 μm is particularly preferred; start timing; stop timing when the surface of the release film is gently wiped with a dry cotton ball without leaving any traces, and record the time, which is the film-forming time of the release agent composition.

[0110] The results show that the film-forming time of the release agent compositions 1-6 on the mold is all within 10 minutes, which shows that the release agent compositions 1-6 can form films in a relatively short time.

[0111] The surface of the release film was photographed with a camera to observe the film-forming state of the release agent composition. The surface of the film formed by the release agent composition was shown in the attached Figure 1 ; Figure 1 It is shown that the release films formed on the mold by the release agent compositions 1-6 all have flat and smooth surfaces.

[0112] Test 4 Demolding properties of release agent compositions 1-6

[0113] The release agent compositions 1-6 prepared in Examples 3-8 were applied to a cleaned mold with a coating thickness of 0.05-5 μm, preferably 0.1-2 μm. Then, 191 unsaturated resin was continuously molded on the mold. The molding process was terminated when the 191 unsaturated resin adhered to the mold or could not be easily removed from the mold. The number of continuous demolding of the 191 unsaturated resin on the release agent compositions 1-6 was recorded respectively. The results are shown in Table 2.

[0114] Table 2 Continuous demoulding times of release agent

[0115] Example Release agent composition Continuous demoulding times / times Film forming properties 3 1 15 whole 4 2 23 whole 5 3 19 whole 6 4 15 whole 7 5 25 whole 8 6 21 whole

[0116] It can be seen from Table 2 that the release agent compositions 1-6 can be demolded on the mold continuously for more than 15-25 times, and the best one is the release agent composition 5, which can be demolded 25 times continuously, which is better than most commercially available silicone release agents.

[0117] Test 5 Thermal stability test of release agent compositions 1-6

[0118] The release agent compositions 1-6 of Examples 3-8 were respectively taken, and the thermal stability of the release agent was tested using a thermogravimetric analyzer. The specific process was as follows:

[0119] Under the protection of N2 atmosphere, release agent compositions 1-6 were placed in crucibles in a heating furnace and heated at 10C·min -1 The temperature was raised from 35°C to 500°C at a rate of 1.5°C to test the mass loss of release agent compositions 1-6 in the temperature range of 35-500°C. The test results are shown in Figure 2 ,from Figure 2 It can be seen that under the condition of 340-370°C, the mass loss of the release agent composition 5 prepared in Example 7 is the lowest and its thermal stability is higher.

[0120] Figure 2 It shows that the release agent compositions 1-6 all have good thermal stability.

[0121] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A visual semi-permanent release agent, characterized in that: The general structural formula of the release agent is as follows: Wherein: the R1-R8 are independent of each other, and R1-R8 are selected from the same or different straight chain or branched alkyl, alkenyl, cycloalkyl or cycloalkenyl, aryl or aromatic hydrocarbon groups; n is an integer of 1-30, and the sum of x+y is an integer of 1-1000.

2. A visual semi-permanent release agent according to claim 1, wherein R1-R8 is selected from C1-C6 alkyl or alkenyl.

3. A visual semi-permanent release agent according to claim 1, characterized in that: The structural formula of the release agent is as follows: Wherein, x+y=an integer of 300-500, and n is an integer of 2-5.

4. A method for preparing a visual semi-permanent release agent according to any one of claims 1 to 3, characterized in that: The reaction process is as follows: It is prepared by polymerization reaction of vinyl-terminated siloxane compounds and tetrazine compounds at 0-80°C.

5. The method for preparing a visual semi-permanent release agent according to claim 4, characterized in that: In the tetrazine compound, n is an integer of 1-30.

6. The method for preparing a visual semi-permanent release agent according to claim 5, characterized in that: n is an integer from 2 to 5.

7. A visual semi-permanent release agent composition, characterized in that: The invention comprises the release agent according to any one of claims 1 to 3 and amino silicone oil.

8. The method for preparing the release agent composition according to claim 7, characterized in that: The vinyl-terminated siloxane compound, tetrazine compound, amino silicone oil and solvent are stirred in a mass volume ratio of 1g: 0.05-0.15g: 0.01-0.05g: 10-100mL to obtain the product.

9. The method for preparing the release agent composition according to claim 8, characterized in that: The mass volume ratio of the vinyl-terminated siloxane compound, the tetrazine compound, the amino silicone oil and the solvent is 1 g: 0.1 g: 0.02 g: 100 mL.

10. Use of the visual semi-permanent release agent according to any one of claims 1 to 3 or the release agent composition according to claim 7 in preparing external release system products.

Citation Information

Patent Citations

  • Mold-releasable curable composition

    CN1671794A

  • Organosilicone emulsion composition

    US20180346661A1

  • Molding process using curable silicone release compositions

    US4244912A