Preparation method of flexible carbon fiber reinforced polyphenylene sulfide composite material laminated plate
By surface treatment of carbon fiber and melt blending with polyphenylene sulfide resin, combined with hot pressing molding process, a flexible carbon fiber reinforced polyphenylene sulfide composite laminate with excellent mechanical and thermal stability properties was prepared, which solved the existing problems. Solve the problem of insufficient material performance and realize the preparation of high-performance composite materials.
Patent Information
- Application Number
- CN202411049878.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing carbon fiber reinforced polyphenylene sulfide composite materials have poor overall performance and are difficult to meet the application requirements of high temperature and corrosion resistance.
High-quality carbon fiber is used for surface treatment and melt-blended with polyphenylene sulfide resin. The flexible carbon fiber-reinforced polyphenylene sulfide composite laminate is prepared through a hot pressing molding process to ensure the full combination and uniform dispersion of carbon fiber and resin.
The mechanical properties and thermal stability of the composite material are improved, its performance under high temperature and repeated loading conditions is enhanced, the service life is extended, and customized flexibility design is achieved by adjusting the process and material combination.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyphenylene sulfide composite materials, and in particular to a method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate. Background Art
[0002] Carbon fiber is a new type of high-performance fiber-reinforced material. It has many excellent properties such as high strength, high modulus, high temperature resistance, wear resistance, corrosion resistance, fatigue resistance, creep resistance, electrical conductivity, thermal conductivity and far-infrared radiation. It can reduce the weight of components in the form of composite materials, thereby improving the technical performance of components. It is now widely used in aerospace, new textile machinery, petrochemical, medical equipment, automobiles, machinery manufacturing, construction industry, stationery, telecommunications, electric heating and other high-tech fields. Its wide application will greatly change our lifestyle and improve our quality of life. Engineering materials composited with carbon fiber are superior to metal materials. Its tensile strength is 3-4 times higher than that of steel, its stiffness is 2-3 times higher, its fatigue resistance is 2 times higher, it is 3-4 times lighter than steel, and its thermal expansion is 4-5 times smaller. Its emergence has given fiber composite materials a broader development and application prospect. As various fiber material reinforcement technologies have gradually become as important as structural design, the development process of carbon fiber materials has attracted the attention of many developed and developing countries.
[0003] Polyphenylene sulfide (PPS) is a semi-crystalline thermoplastic polymer with high temperature resistance and corrosion resistance, and its melting temperature (Tm) is about 285°C. At present, PPS is used in various industries, but the main chain of PPS contains benzene rings, the whole molecule has a rigid structure, and the sulfur atom at the para position of the benzene ring is unstable, and the bond energy of CS is low. Usually, pure PPS will show shortcomings such as brittleness and easy oxidation, so PPS needs to be modified to improve its performance. At present, the research on PPS modification is mainly carried out from two aspects. On the one hand, chemical modification is carried out to reshape the structure at the molecular level and reduce the introduction of side chains, which can improve the overall performance of the matrix. However, this method is difficult, the matrix performance is not easy to control continuously, and it is time-consuming and labor-intensive. On the other hand, physical modification is carried out to evenly disperse the filler into the PPS matrix by melt blending, so as to achieve the purpose of improving the performance of PPS. In the prior art, polyphenylene sulfide is modified with carbon fiber to give it high temperature resistance, corrosion resistance and other properties. However, the comprehensive performance of the modified polyphenylene sulfide is poor, which is not conducive to application. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate, which solves the problem of poor comprehensive performance.
[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate comprises the following steps: S1: Raw material preparation Select high-quality carbon fiber to ensure that its fiber length, diameter and performance meet the requirements; S2: Carbon fiber pretreatment Surface treatment of carbon fibers, such as chemical oxidation or plasma treatment, to increase surface roughness and activity and improve bonding with polyphenylene sulfide; S3: Resin preparation The polyphenylene sulfide resin is heated to a certain temperature to melt it, and appropriate additives such as lubricants, antioxidants, etc. are added to improve the performance of the composite material; S4: Impregnation process The pretreated carbon fiber bundle or fabric is impregnated in the prepared polyphenylene sulfide resin to ensure that the carbon fiber is fully impregnated with the resin; S5: Layering The impregnated carbon fiber and polyphenylene sulfide resin are stacked and laid in accordance with a predetermined laying order and angle; S6: Thermoforming The laminated materials are placed in a hot press and hot pressed under certain temperature, pressure and time conditions to fully cure the resin and form a laminate. S7: Cooling and demoulding After the hot pressing is completed, the laminate is allowed to cool naturally to room temperature in the mold and then demolded and taken out; S8: Post-processing The prepared laminates are post-processed by cutting, grinding, etc. to obtain the required size and surface quality.
[0006] Preferably, in step S1, high-strength, high-modulus carbon fibers, such as T300, T700 or T800, are selected, and the diameter of the fibers is usually between 5 and 8 microns to ensure good mechanical properties and reinforcement effects.
[0007] Preferably, in step S2, the carbon fiber pretreatment includes surface cleaning, oxidation treatment, plasma treatment, coating treatment and ultrasonic treatment.
[0008] Preferably, in step S3, the polyphenylene sulfide resin particles or powder are placed in a heating device, such as an oven or a heating kettle, and the temperature is gradually raised to above its melting point, usually between 280-300°C, so that the resin is completely melted, and a mechanical stirrer or a magnetic stirrer is used to fully stir the molten resin and additives at an appropriate speed to ensure that the various components are evenly distributed. The stirring time is usually 30-60 minutes.
[0009] Preferably, in step S4, the prepared polyphenylene sulfide resin is heated to a suitable impregnation temperature, usually between 280-320° C., so that the resin maintains good fluidity, and the impregnation time is generally 30 minutes to 2 hours.
[0010] Preferably, in step S6, the hot pressing temperature is set between 280-350° C., the pressure is generally within the range of 5-20 MPa, and the duration is usually 1-3 hours.
[0011] The present invention provides a method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate, which has the following beneficial effects: The present invention combines the high strength and high modulus properties of carbon fiber with the excellent chemical stability and high temperature resistance of polyphenylene sulfide, so that the laminate has excellent mechanical properties and thermal stability. The low density of carbon fiber reduces the weight of the laminate while ensuring the strength. The composite laminate can maintain good performance and extend the service life under repeated loading and unloading.
[0012] The present invention can achieve customized design of laminate performance by adjusting the plying sequence, angle and content of carbon fibers, as well as the formula of polyphenylene sulfide resin, and adopts specific process and material combination to effectively improve the flexibility of the laminate, so that it performs well in applications that require bending and deformation. DETAILED DESCRIPTION
[0013] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0014] An embodiment of the present invention provides a method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate, comprising the following steps: S1: Raw material preparation Select high-quality carbon fiber to ensure that its fiber length, diameter and performance meet the requirements; S2: Carbon fiber pretreatment Surface treatment of carbon fibers, such as chemical oxidation or plasma treatment, to increase surface roughness and activity and improve bonding with polyphenylene sulfide; S3: Resin preparation The polyphenylene sulfide resin is heated to a certain temperature to melt it, and appropriate additives such as lubricants, antioxidants, etc. are added to improve the performance of the composite material; S4: Impregnation process The pretreated carbon fiber bundle or fabric is impregnated in the prepared polyphenylene sulfide resin to ensure that the carbon fiber is fully impregnated with the resin; S5: Layering The impregnated carbon fiber and polyphenylene sulfide resin are stacked and laid in accordance with a predetermined laying order and angle; S6: Thermoforming The laminated materials are placed in a hot press and hot pressed under certain temperature, pressure and time conditions to fully cure the resin and form a laminate. S7: Cooling and demoulding After the hot pressing is completed, the laminate is allowed to cool naturally to room temperature in the mold and then demolded and taken out; S8: Post-processing The prepared laminates are post-processed by cutting, grinding, etc. to obtain the required size and surface quality.
[0015] In step S1, high-strength, high-modulus carbon fiber, such as T300 model, is selected, and the diameter of the fiber is usually 5 microns to ensure good mechanical properties and reinforcement effect; Make sure the length of the carbon fiber is selected according to specific needs. Short-cut carbon fiber is suitable for certain injection molding processes, while continuous carbon fiber is more suitable for the preparation of composite panels.
[0016] In step S2, the carbon fiber pretreatment includes surface cleaning, oxidation treatment, plasma treatment, coating treatment and ultrasonic treatment; Surface cleaning: remove impurities and contaminants on the surface of carbon fiber by cleaning to improve the bonding force between carbon fiber and matrix material; Oxidation treatment: Use an oxidant to treat the surface of the carbon fiber to increase the number of oxygen-containing functional groups on the surface of the carbon fiber, thereby improving the chemical bonding between the carbon fiber and the matrix material; Plasma treatment: Use high-energy particles of plasma to bombard and etch the surface of carbon fiber, change the chemical structure and physical properties of the carbon fiber surface, and improve the interface bonding strength between carbon fiber and matrix material; Coating treatment: Apply an organic or inorganic coating on the surface of the carbon fiber to improve the compatibility and adhesion between the carbon fiber and the matrix material; Ultrasonic treatment: Use the cavitation effect and mechanical vibration of ultrasound to clean and activate the carbon fiber surface to improve the interface bonding strength between the carbon fiber and the matrix material.
[0017] In step S3, polyphenylene sulfide resin particles or powder are placed in a heating device, such as an oven or a heating kettle, and the temperature is gradually raised to above its melting point, usually 280° C., so that the resin is completely melted, and a mechanical stirrer or a magnetic stirrer is used to fully stir the molten resin and the additive at an appropriate speed to ensure that the various components are evenly distributed. The stirring time is usually 30 minutes; Toughening agents: For example, thermoplastic elastomers (such as SEBS or EVA) can improve the toughness and impact resistance of composite materials.
[0018] Lubricants: Such as silicone oil or zinc stearate, which help reduce friction between the resin and the mold or equipment during processing, and improve the fluidity and surface quality of the material.
[0019] Antioxidants: such as hindered phenols (such as BHT) or phosphite antioxidants, which prevent polyphenylene sulfide from oxidative degradation during high-temperature processing and use, thereby extending the service life of the material.
[0020] In step S4, the prepared polyphenylene sulfide resin is heated to a suitable impregnation temperature, usually between 280° C., so that the resin maintains good fluidity. The impregnation time is generally 30 minutes.
[0021] In step S6, the hot pressing temperature is set at 280°C, the pressure is generally set at 5 MPa, and the duration is usually 1 hour. Example
[0022] An embodiment of the present invention provides a method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate, comprising the following steps: S1: Raw material preparation Select high-quality carbon fiber to ensure that its fiber length, diameter and performance meet the requirements; S2: Carbon fiber pretreatment Surface treatment of carbon fibers, such as chemical oxidation or plasma treatment, to increase surface roughness and activity and improve bonding with polyphenylene sulfide; S3: Resin preparation The polyphenylene sulfide resin is heated to a certain temperature to melt it, and appropriate additives such as lubricants, antioxidants, etc. are added to improve the performance of the composite material; S4: Impregnation process The pretreated carbon fiber bundle or fabric is impregnated in the prepared polyphenylene sulfide resin to ensure that the carbon fiber is fully impregnated with the resin; S5: Layering The impregnated carbon fiber and polyphenylene sulfide resin are stacked and laid in accordance with a predetermined laying order and angle; S6: Thermoforming The laminated materials are placed in a hot press and hot pressed under certain temperature, pressure and time conditions to fully cure the resin and form a laminate. S7: Cooling and demoulding After the hot pressing is completed, the laminate is allowed to cool naturally to room temperature in the mold and then demolded and taken out; S8: Post-processing The prepared laminates are post-processed by cutting, grinding, etc. to obtain the required size and surface quality.
[0023] In step S1, high-strength, high-modulus carbon fibers, such as T800, are selected. The diameter of the fibers is usually between 8 microns to ensure good mechanical properties and reinforcement effects.
[0024] In step S2, the carbon fiber pretreatment includes surface cleaning, oxidation treatment, plasma treatment, coating treatment and ultrasonic treatment.
[0025] In step S3, polyphenylene sulfide resin particles or powder are placed in a heating device, such as an oven or a heating kettle, and the temperature is gradually raised to above its melting point, usually between 300°C, so that the resin is completely melted. A mechanical stirrer or a magnetic stirrer is used to fully stir the molten resin and additives at an appropriate speed to ensure that the various components are evenly distributed. The stirring time is usually 60 minutes.
[0026] In step S4, the prepared polyphenylene sulfide resin is heated to a suitable impregnation temperature, usually 320° C., so that the resin maintains good fluidity. The impregnation time is generally 2 hours.
[0027] In step S6, the hot pressing temperature is set at 350°C, the pressure is generally within 20 MPa, and the duration is usually 3 hours.
[0028] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate, characterized in that: The following steps are involved: S1: Raw material preparation Select high-quality carbon fiber to ensure that its fiber length, diameter and performance meet the requirements; S2: Carbon fiber pretreatment Surface treatment of carbon fibers, such as chemical oxidation or plasma treatment, to increase surface roughness and activity and improve bonding with polyphenylene sulfide; S3: Resin preparation The polyphenylene sulfide resin is heated to a certain temperature to melt it, and appropriate additives such as lubricants, antioxidants, etc. are added to improve the performance of the composite material; S4: Impregnation process The pretreated carbon fiber bundle or fabric is impregnated in the prepared polyphenylene sulfide resin to ensure that the carbon fiber is fully impregnated with the resin; S5: Layering The impregnated carbon fiber and polyphenylene sulfide resin are stacked and laid in accordance with a predetermined laying order and angle; S6: Thermoforming The laminated materials are placed in a hot press and hot pressed under certain temperature, pressure and time conditions to fully cure the resin and form a laminate. S7: Cooling and demoulding After the hot pressing is completed, the laminate is allowed to cool naturally to room temperature in the mold and then demolded and taken out; S8: Post-processing The prepared laminates are post-processed by cutting, grinding, etc. to obtain the required size and surface quality.
2. The method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate according to claim 1, characterized in that: In step S1, high-strength, high-modulus carbon fibers, such as T300, T700 or T800, are selected. The diameter of the fibers is usually between 5 and 8 microns to ensure good mechanical properties and reinforcement effects.
3. The method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate according to claim 1, characterized in that: In step S2, the carbon fiber pretreatment includes surface cleaning, oxidation treatment, plasma treatment, coating treatment and ultrasonic treatment.
4. The method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate according to claim 1, characterized in that: In step S3, polyphenylene sulfide resin particles or powder are placed in a heating device, such as an oven or a heating kettle, and the temperature is gradually raised to above its melting point, usually between 280-300°C, so that the resin is completely melted. A mechanical stirrer or a magnetic stirrer is used to fully stir the molten resin and additives at an appropriate speed to ensure that the various components are evenly distributed. The stirring time is usually 30-60 minutes.
5. The method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate according to claim 1, characterized in that: In step S4, the prepared polyphenylene sulfide resin is heated to a suitable impregnation temperature, usually between 280-320° C., so that the resin maintains good fluidity. The impregnation time is generally 30 minutes to 2 hours.
6. The method for preparing a flexible carbon fiber reinforced polyphenylene sulfide composite laminate according to claim 1, characterized in that: In step S6, the hot pressing temperature is set between 280-350°C, the pressure is generally within the range of 5-20 MPa, and the duration is usually 1-3 hours.
Citation Information
Cited By
Preparation method of fiber cloth reinforced polyphenylene sulfide alloy prepreg sheet, composite board and preparation method and application of composite board
CN120588531A
Chopped carbon fiber reinforced polyphenylene sulfide pre-composite powder and preparation method thereof
CN121825005A