Wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate

By using hydrofluoric acid and sodium sulfate as joint precipitants in wet phosphoric acid, and adding flocculants, the removal rate of magnesium and aluminum ions and the yield of phosphoric acid are significantly improved, solving the problem of low removal rate of magnesium and aluminum metal ions in wet phosphoric acid. To solve the problem of insufficient phosphoric acid yield, an efficient wet phosphoric acid purification process has been realized.

CN118723952APending Publication Date: 2024-10-01GUIZHOU CHANHEN CHEM CO LTD +1

Patent Information

Application Number
CN202410853263.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The removal rate of magnesium and aluminum metal ions in existing wet phosphoric acid is not high, and the traditional chemical precipitation method has problems with impurity residues and low phosphoric acid yield, making it difficult to meet the demand for high-quality purification.

Method used

Hydrofluoric acid and sodium sulfate are used as joint precipitants, combined with carboxymethyl cellulose, cationic polyacrylamide, anionic polyacrylamide or zwitterionic polyacrylamide as flocculants, to precipitate and settle at a specific temperature, significantly accelerating precipitation. speed and phosphoric acid yield.

Benefits of technology

It achieves high magnesium and aluminum ion removal rate and high phosphoric acid yield, reducing losses and improving product quality. The phosphoric acid yield can reach more than 70%, which is much higher than the traditional method of about 70%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723952A_ABST
    Figure CN118723952A_ABST
Patent Text Reader

Abstract

The invention discloses a wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate. The method comprises the following steps: by taking hydrofluoric acid and sodium sulfate as a combined precipitant and one of carboxymethyl cellulose, cationic polyacrylamide, anionic polyacrylamide or zwitterionic polyacrylamide as a flocculating agent, firstly adding the flocculating agent at 40-80 DEG C, then adding the combined precipitant, and precipitating a wet-process phosphoric acid solution, and then aging at the temperature of 35-45 DEG C. The process disclosed by the invention has the characteristics of few newly introduced impurity ions, diversified precipitant functions, high precipitation speed and high phosphoric acid yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a process for removing impurity ions of wet-process magnesium aluminum phosphate, and a wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium aluminum ion removal rate. Background Art

[0002] Phosphoric acid is a global strategic resource related to the national livelihood security. With the rapid development of science and technology, the demand for phosphoric acid is increasing. The wet process can efficiently and fully extract phosphoric acid from low-grade phosphate ore, and has become the main method for producing phosphoric acid in my country. However, there are a large number of magnesium and aluminum metal ion impurities in wet phosphoric acid, which inhibits the use of wet phosphoric acid. Therefore, removing magnesium and aluminum metal ion impurities in wet phosphoric acid is of great significance to my country's phosphorus chemical industry.

[0003] At present, the main methods for removing magnesium and aluminum metal ion impurities in wet-process phosphoric acid include ion exchange, membrane separation, solvent extraction and chemical precipitation, etc. Among them, chemical precipitation is a simple and low-cost technology, which is particularly suitable for pre-purification before deep processing of wet-process phosphoric acid.

[0004] The traditional chemical precipitation method uses hydrofluoric acid as a precipitant. Fluorine can combine with metal ion impurities to form precipitation to a certain extent, thereby achieving the removal of metal ion impurities. However, the removal rate is not high and cannot meet the needs of high-quality wet phosphoric acid purification. To this end, some researchers introduced sodium chloride or sodium carbonate into hydrofluoric acid and used it as a co-precipitant with hydrofluoric acid to form NaMgAlF6 precipitation with metal ions, thereby further improving the removal rate of magnesium and aluminum metal ion impurities.

[0005] Although this improved precipitation method has improved the removal rate of magnesium and aluminum metal ion impurities to a certain extent, it still has many defects: 1. The introduced chloride ions are difficult to remove, and the chloride ion impurities formed will seriously affect the quality of downstream phosphoric acid products. 2. Carbonate ions cannot coexist under acidic conditions and their role is limited. 3. Regardless of whether sodium chloride or sodium carbonate is introduced, the particle size of the formed NaMgAlF6 is very small, which is difficult to precipitate and separate. It takes dozens of days of natural aging to achieve a higher phosphoric acid yield, but the maximum phosphoric acid yield of this precipitation method can only reach about 70%, which causes great losses when implemented in industry.

[0006] The flocculant sedimentation method is a method of using flocculants to precipitate particles in a solution. It is also used in a small amount in the process of removing impurities from wet-process phosphoric acid. For example, Wang Yonggui et al. reported the process of removing impurities from wet-process phosphoric acid using flocculants in the document "Sedimentation Characteristics of Impurity Particles in Concentrated Wet-Process Phosphoric Acid". However, the current flocculant sedimentation method is mainly aimed at the precipitation of particles in wet-process phosphoric acid after it is produced, and cannot remove magnesium and aluminum metal ions in wet-process phosphoric acid. The researchers found that when the magnesium and aluminum metal ions in wet-process phosphoric acid are precipitated by chemical precipitation to form a precipitate and then a flocculant is added for sedimentation, although it can accelerate sedimentation to a certain extent, the phosphoric acid yield after rapid sedimentation decreases and the loss rate increases, causing considerable losses to production companies.

[0007] Therefore, improving the removal process of impurity ions of magnesium aluminum phosphate in wet process, accelerating the formation of precipitation, and increasing the yield of phosphoric acid are technical problems that must be solved in the current wet process phosphoric acid purification process. Summary of the invention

[0008] In order to solve the above technical problems, the present invention provides a wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate. The process of the present invention has the characteristics of less newly introduced impurity ions, diverse precipitation agent functions, fast precipitation speed and high phosphoric acid yield.

[0009] The technical solution of the present invention:

[0010] A wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, which uses hydrofluoric acid and sodium sulfate as joint precipitants, uses one or more of carboxymethyl cellulose, cationic polyacrylamide, anionic polyacrylamide or zwitterionic polyacrylamide as flocculants, first adds the flocculant at 40-80°C, then adds the joint precipitant, precipitates the wet phosphoric acid solution, and then ages it at 35-45°C.

[0011] Preferably, the aforementioned wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate comprises the following specific steps:

[0012] S1. After the wet-process phosphoric acid solution is taken out, the temperature is maintained at 40-80°C;

[0013] S2. Add carboxymethyl cellulose, cationic polyacrylamide, anionic polyacrylamide or zwitterionic polyacrylamide as a flocculant to the wet-process phosphoric acid solution of S1, maintain the temperature unchanged, and react for 20-40 minutes to obtain a crude product;

[0014] S3. Add hydrofluoric acid and sodium sulfate to the crude product of S2, maintain the temperature unchanged, and continue the reaction for 20-40 minutes. After the reaction, a suspension is obtained;

[0015] S4. Lower the temperature of the suspension of S3 to 35-45°C and age it for 1-7 days.

[0016] Preferably, in the aforementioned wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the temperature in S1 is maintained at 60° C. 60° C. is the normal insulation temperature of wet-process phosphoric acid after production, and carrying out the reaction at this temperature can avoid energy loss.

[0017] Preferably, in the aforementioned wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the flocculant in S2 is carboxymethyl cellulose.

[0018] Preferably, in the aforementioned wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the flocculant in S2 needs to be configured into an aqueous solution with a mass concentration of 0.05-0.15% before use, and then added to the wet-process phosphoric acid solution, wherein the mass ratio of the aqueous solution to the wet-process phosphoric acid solution is 3-5:100.

[0019] Preferably, in the aforementioned wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the mass concentration of the flocculant in the aqueous solution is 0.1%, and the mass ratio of the aqueous solution to the wet-process phosphoric acid solution is 4:100.

[0020] Preferably, in the aforementioned wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the mass ratio of the crude product, hydrofluoric acid and sodium sulfate in S3 is 200:10-30:5-20.

[0021] Preferably, in the aforementioned wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the mass ratio of the crude product, hydrofluoric acid and sodium sulfate is 200:26:16.

[0022] Preferably, in the aforementioned wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the reactions in S2 and S3 are carried out under stirring conditions with a stirring rate of 100-300 r / min.

[0023] Preferably, in the aforementioned wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the temperature of the suspension in S4 is reduced to 40° C. and then aged.

[0024] Beneficial effects of the present invention:

[0025] 1. The precipitating agents of the present invention are hydrofluoric acid and sodium sulfate. In addition to conventional hydrofluoric acid, the introduction of sodium sulfate does not bring new impurities, which is more conducive to ensuring the quality of wet-process phosphoric acid. At the same time, in addition to providing sodium ions to form NaMgAlF6 precipitation, the sulfate radicals in the sodium sulfate of the present invention can also combine with calcium ions in the wet-process phosphoric acid to form a stable calcium sulfate precipitation, thereby further removing calcium ion impurities in the wet-process phosphoric acid and achieving multiple functions.

[0026] 2. The present invention greatly accelerates the agglomeration and sedimentation of NaMgAlF6 precipitate by adding flocculants. After aging for 2-5 days, the yield of phosphoric acid can reach more than 70%, and can reach a maximum of more than 90%, which is much higher than the current maximum phosphoric acid yield of about 70% by the chemical precipitation method.

[0027] 3. The present invention first adds a flocculant and then adds a combined precipitant for reaction and sedimentation. Compared with the method of first reacting with a precipitant and then adding a flocculant, the method of the present invention has a higher yield and a lower loss rate of the phosphoric acid solution, which can reduce losses for production enterprises. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Attached Figure 1 The figure is a comparison chart of the effects of different aging temperatures and times on phosphoric acid yield and turbidity removal rate of the present invention.

[0029] Attached Figure 2 The polarized light microscope images of the floccules of the present invention in the process of flocculation followed by precipitation and precipitation followed by flocculation are shown. It can be seen that when standing for 0 days, compared with the flocculation method of precipitation followed by flocculation, the suspended particles in the phosphoric acid solution of flocculation followed by precipitation are more aggregated. Therefore, under the same standing time, the phosphoric acid yield and turbidity removal rate of flocculation followed by precipitation are higher than those of precipitation followed by flocculation. After standing for 0.5 days, the phosphoric acid solutions of the two flocculation methods show the phenomenon of small particle floccules agglomerating with each other to form larger agglomerates. When the time is further extended to 3.5 days, no particles to be settled are observed in the phosphoric acid solution. This is because the large particle agglomerates formed under the flocculation action settle in large quantities due to gravity, and the phosphoric acid yield and turbidity removal rate are relatively high at this time.

[0030] Figure 3 The particle size distribution diagram of the present invention is first flocculation and then precipitation and first precipitation and then flocculation. It can be seen that the D of the flocs obtained by first flocculation and then precipitation is 50 The median diameter is 52.86 μm; the D of the flocs obtained by precipitation followed by flocculation 50 This further shows that the method of flocculation followed by sedimentation can form floccules with larger particle size, thereby improving the sedimentation efficiency.

[0031] Figure 4The Zeta potential diagram of flocs formed by different flocculation and sedimentation methods. It can be seen that when the flocculation method of flocculation first and then sedimentation is adopted, the Zeta potential of the flocs is 1.57mV; when the flocculation method of sedimentation first and then flocculation is adopted, the Zeta potential of the flocs is 1.76mV. Compared with the former, the Zeta potential of the latter is increased, which indicates that when the method of flocculation first and then sedimentation is adopted, the electrostatic repulsion between the flocculation system and NaMgAlF6·H2O(s) is smaller, it is easier to agglomerate, and the floc particle size is larger. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.

[0033] Embodiment 1 of the present invention

[0034] A wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the specific steps are as follows:

[0035] S1. Weigh 200 g of the wet-process phosphoric acid solution and maintain the temperature at 60°C;

[0036] S2. Add 8 g of 0.1% carboxymethyl cellulose aqueous solution as a flocculant to the wet-process phosphoric acid solution of S1, maintain the temperature unchanged, and react for 30 min to obtain a crude product;

[0037] S3. Add 26 g of hydrofluoric acid and 16 g of sodium sulfate to the crude product of S2, maintain the temperature, and continue the reaction for 30 min. After the reaction, a suspension is obtained;

[0038] S4. Lower the temperature of the suspension of S3 to 40°C and age it for 3 days.

[0039] Embodiment 2 of the present invention

[0040] A wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the specific steps of the method are as follows:

[0041] S1. Weigh 200 g of the wet-process phosphoric acid solution and maintain the temperature at 40°C;

[0042] S2. Add 6 g of a 0.15% cationic polyacrylamide aqueous solution as a flocculant to the wet-process phosphoric acid solution of S1, maintain the temperature unchanged, and react for 20 min to obtain a crude product;

[0043] S3. Add 10 g of hydrofluoric acid and 5 g of sodium sulfate to the crude product of S2, maintain the temperature, and continue the reaction for 20 min. After the reaction, a suspension is obtained;

[0044] S4. Lower the temperature of the suspension in S3 to 35°C and age it for 7 days.

[0045] Embodiment 3 of the present invention

[0046] A wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the specific steps of the method are as follows:

[0047] S1. Weigh 200 g of the wet-process phosphoric acid solution and maintain the temperature at 80 ° C;

[0048] S2. Add 10 g of anionic polyacrylamide with a mass concentration of 0.15% as a flocculant to the wet-process phosphoric acid solution of S1, maintain the temperature unchanged, and react for 40 minutes to obtain a crude product;

[0049] S3. Add 30 g of hydrofluoric acid and 20 g of sodium sulfate to the crude product of S2, maintain the temperature, and continue the reaction for 40 min. After the reaction, a suspension is obtained;

[0050] S4. Lower the temperature of the suspension in S3 to 45°C and age it for 1 day.

[0051] Embodiment 4 of the present invention

[0052] A wet phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, the specific steps of the method are as follows:

[0053] S1. Weigh 200 g of the wet-process phosphoric acid solution and maintain the temperature at 60°C;

[0054] S2. Add 8 g of zwitterionic polyacrylamide with a mass concentration of 0.1% as a flocculant to the wet-process phosphoric acid solution of S1, maintain the temperature unchanged, and react for 30 minutes to obtain a crude product;

[0055] S3. Add 25 g of hydrofluoric acid and 15 g of sodium sulfate to the crude product of S2, maintain the temperature, and continue the reaction for 30 min. After the reaction, a suspension is obtained;

[0056] S4. Lower the temperature of the suspension of S3 to 40°C and age it for 5 days.

[0057] Experimental Example 1:

[0058] The applicant studied the phosphoric acid yield of different flocculants, and the experimental route is as follows:

[0059] The composition of the wet-process phosphoric acid stock solution used in this experiment is shown in Table 1:

[0060] Table 1 Composition of wet process phosphoric acid stock solution

[0061] Components Content (wt%) <![CDATA[P2O5]]> 35.42 MgO 1.92 <![CDATA[Al2O3]]> 2.34

[0062] S1. After the wet phosphoric acid solution is taken out, 5 portions of 200 g of the wet phosphoric acid solution are weighed and the temperature is maintained at 60° C., which is the temperature range for the production of the wet phosphoric acid solution and subsequent constant temperature storage;

[0063] S2. Add the following to 5 parts of wet-process phosphoric acid solution of S1: a. without adding auxiliary coagulant; b. adding 8g of 0.1% carboxymethyl cellulose aqueous solution; c. adding 8g of 0.1% cationic polyacrylamide aqueous solution; d. adding 8g of 0.1% anionic polyacrylamide aqueous solution; e. adding 8g of 0.1% zwitterionic polyacrylamide aqueous solution; maintaining the temperature unchanged, reacting for 30min respectively to obtain a crude product;

[0064] S3. To the crude product of S2, 26 g of hydrofluoric acid and 16 g of sodium sulfate were added respectively, the temperature was maintained constant, and the reaction was continued for 30 min. After the reaction, a suspension was obtained;

[0065] S4. The temperature of the suspension of S3 is reduced to 40°C and aged for 1-10 days;

[0066] S5. According to the phosphoric acid yield formula as shown in Formula 1:

[0067]

[0068] Where: m i ——Mass of phosphoric acid before impurity removal, g; m f ——Mass of phosphoric acid after impurity removal, g. The phosphoric acid yield of 5 parts of wet-process phosphoric acid was calculated, and the results are shown in Table 2.

[0069] Table 2 Phosphoric acid yield statistics

[0070]

[0071] As can be seen from Table 2, the removal rates of metal ions before and after the addition of flocculants are similar, and both can achieve a high metal ion removal rate. However, without the addition of flocculants, the yield of phosphoric acid is very low at 60°C, and the yield of phosphoric acid after aging for 10 days is only 20%. After the addition of flocculants, the yield of phosphoric acid increases significantly, and can reach more than 70% within 2-5 days, and the highest yield after aging for 10 days can reach 96%.

[0072] Experimental Example 2:

[0073] The applicant has studied the yield of phosphoric acid after aging at different temperatures, and the experimental method is as follows:

[0074] According to the process route of Example 1, the experiment was carried out, and the aging temperature was changed to 25°C, 30°C, 40°C, 50°C and 60°C respectively. The effects of different aging temperatures on the phosphoric acid yield and phosphoric acid turbidity removal rate during the NaMgAlF6 precipitation process were compared. The experimental results are as follows: Figure 1 shown.

[0075] Depend on Figure 1 (a) It can be seen that the precipitation effect of carboxymethyl cellulose on NaMgAlF6 is different at different aging temperatures. When the temperature is lower than 40°C, the phosphoric acid yield increases with the increase of temperature. However, when the temperature is higher than 40°C, the phosphoric acid yield decreases slightly. For example, when the aging temperature is 25°C, 30°C, 40°C and 50°C, the time required for the phosphoric acid yield to reach more than 70% is 5 days, 3 days, 2 days and 5 days respectively. When the aging temperature is 60°C, the phosphoric acid yield is always lower than 70% during the aging period of 7 days. It shows that when the temperature is lower than 40°C, the phosphoric acid yield increases with the increase of temperature. However, when the temperature is higher than 40°C, the phosphoric acid yield decreases slightly.

[0076] Depend on Figure 1 (b) It can be seen that when the aging temperature is 25℃, 30℃, 40℃, 50℃ and 60℃, the time required for the turbidity removal rate to reach about 90% is 3 days, 3 days, 2.5 days, 7 days and 7 days respectively. After aging for 7 days, in the temperature range of 40-60℃, the turbidity removal rate dropped from 99.7% to 76.3%. This is because the higher the temperature, the more energy is provided, and the easier it is for the flocculant to form flocs with NaMgAlF6. However, when the temperature is too high, the particles move too fast in the reaction system, forming flocs with smaller particle size, causing hydration.

[0077] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate, characterized in that: Hydrofluoric acid and sodium sulfate are used as joint precipitants, and one of carboxymethyl cellulose, cationic polyacrylamide, anionic polyacrylamide or zwitterionic polyacrylamide is used as a flocculant. The flocculant is first added at 40-80°C, and then the joint precipitant is added to precipitate the wet-process phosphoric acid solution, and then the solution is aged at 35-45°C.

2. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 1, characterized in that: The specific steps of the method are as follows: S1. After the wet-process phosphoric acid solution is taken out, the temperature is maintained at 40-80°C; S2. Add one or more of carboxymethyl cellulose, cationic polyacrylamide, anionic polyacrylamide or zwitterionic polyacrylamide as flocculants to the wet-process phosphoric acid solution of S1, maintain the temperature unchanged, and react for 20-40 minutes to obtain a crude product; S3. Add hydrofluoric acid and sodium sulfate to the crude product of S2, maintain the temperature unchanged, and continue the reaction for 20-40 minutes. After the reaction, a suspension is obtained; S4. Lower the temperature of the suspension of S3 to 35-45°C and age it for 1-7 days.

3. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 2, characterized in that: S1 The temperature is maintained at 60°C.

4. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 2, characterized in that: S2 The flocculant is carboxymethyl cellulose.

5. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 2, characterized in that: S2 The flocculant needs to be prepared into an aqueous solution with a mass concentration of 0.05-0.15% before use, and then added to the wet-process phosphoric acid solution, wherein the mass ratio of the aqueous solution to the wet-process phosphoric acid solution is 3-5:

100.

6. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 5, characterized in that: The mass concentration of the flocculant in the aqueous solution is 0.1%, and the mass ratio of the aqueous solution to the wet-process phosphoric acid solution is 4:

100.

7. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 2, characterized in that: The mass ratio of the crude product, hydrofluoric acid and sodium sulfate in S3 is 200:10-30:5-20.

8. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 7, characterized in that: The mass ratio of the crude product, hydrofluoric acid and sodium sulfate is 200:26:

16.

9. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 2, characterized in that: The reactions in S2 and S3 are carried out under stirring conditions with a stirring rate of 100-300 r / min.

10. The wet-process phosphoric acid purification process with high phosphoric acid yield and high magnesium and aluminum ion removal rate according to claim 2, characterized in that: S4: the temperature of the suspension is lowered to 40°C and then aged.

Citation Information

Patent Citations

  • Flocculant suitable for wet phosphoric acid production, and impurity sedimentation system

    CN110548317A

  • Process for the removal of heavy metals from a phosphoric acid containing composition using a flocculating agent

    EP3964476A1

  • Process for producing wet process phosphoric acid from phosphate rocks containing fluochlorapatite and related minerals

    US4485078A

  • Process of removing cationic impurities from wet process phosphoric acid

    US4639359A

Cited By

  • Method for purifying and removing impurities in wet-process phosphoric acid

    CN121134705A