Monodisperse long-life room-temperature phosphorescent carbon dot-silica microsphere and preparation method thereof

Monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres were prepared through in-situ synthesis using glucose, PVP and TEOS, which solved the problems of complex embedding of carbon dots in silica microspheres and short phosphorescence lifetime in the existing technology. , achieving an efficient and simple preparation process and long-life phosphorescence effect, which is suitable for information encryption and other fields.

CN118724003APending Publication Date: 2024-10-01UNIV OF JINAN

Patent Information

Application Number
CN202410955143.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, the method of achieving long-life room temperature phosphorescence with carbon dots in monodispersed silica microspheres is complicated and has a short phosphorescence lifetime, and it is difficult to obtain uniform monodispersed carbon dots@silica microspheres, which limits its application.

Method used

Glucose, polyvinylpyrrolidone (PVP), ammonia and ethyl orthosilicate (TEOS) are used as raw materials to prepare monodispersed long-life room temperature phosphorescent carbon dots@silica microspheres through in-situ synthesis. The process includes ethanol and water. Glucose and PVP are added to the mixed solution, TEOS is added, stirred and calcined, and high-speed centrifugation and high-temperature reactors are used to achieve uniform embedding and stabilization of carbon dots.

Benefits of technology

A simple and easy preparation of monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres has been achieved. The phosphorescence lifetime reaches 1.05 seconds and can last for 16 seconds with the naked eye after turning off the UV lamp. It is suitable for industrial production and information encryption applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724003A_ABST
    Figure CN118724003A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: adding glucose and PVP (Polyvinyl Pyrrolidone) into a mixed solution of ethanol and water, adding ammonia water into the mixed solution, stirring to obtain a transparent solution, adding TEOS (Tetraethyl Orthosilicate), stirring, carrying out hydrothermal treatment, centrifuging, drying, and calcining in a muffle furnace to obtain the monodisperse long-life room-temperature phosphorescent carbon dot-coated silicon dioxide microspheres. The monodisperse long-service-life room-temperature phosphorescent carbon dot-silicon dioxide microspheres are obtained. The preparation method is characterized in that monodisperse long-life room-temperature phosphorescent carbon dot-silica microspheres are directly obtained through an in-situ synthesis method. Besides, the monodisperse long-life room-temperature phosphorescent carbon dot-silicon dioxide microspheres synthesized in situ have bright yellow phosphorescence and good monodispersity, the average phosphorescence life of the obtained monodisperse long-life room-temperature phosphorescent carbon dot-silicon dioxide microspheres is 1.05 s, and the phosphorescence with dynamic color change from yellow to green can be seen for 16 s by naked eyes after an ultraviolet lamp is turned off. The medicines used for preparation are cheap and easy to obtain, the preparation process is simple and convenient, and complicated and tedious post-treatment steps are not needed. The prepared monodisperse long-life room-temperature phosphorescent carbon dot-silica microspheres can be successfully applied to the fields of information encryption and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon dot material preparation, and specifically relates to a monodisperse long-life room temperature phosphorescent carbon dot@silica microsphere and a preparation method thereof. Background Art

[0002] Monodisperse silica microspheres have great application prospects in environmental protection, biomedicine, pharmaceutical preparations and information encryption due to their good dispersibility, large specific surface area and excellent chemical stability. Recently, monodisperse silica microspheres with long-life room temperature phosphorescence have been successfully prepared by introducing room temperature phosphorescent materials into monodisperse silica microspheres, which has attracted widespread attention from researchers. At present, commonly used phosphorescent materials are mainly composed of pure organic compounds based on molecular design and inorganic complexes designed based on transition metals and rare earth ions. Among them, carbon dots, as a new type of room temperature phosphorescent nanomaterials, are considered to be suitable candidates for constructing long-life room temperature phosphorescent materials due to their advantages such as simple preparation process, good luminescence performance and low toxicity. However, due to the problems of non-radiative transition of triplet excitons and environment-induced quenching, it is still an important challenge to achieve long-life room temperature phosphorescence of carbon dots. In existing reports, the generation and stabilization of triplet excitons have been successfully achieved through protection by rigid matrices (such as silica, etc.). However, there are few reports on embedding carbon dots into monodisperse silica microspheres to achieve long-life room temperature phosphorescence.

[0003] Although monodisperse room temperature phosphorescent carbon dots@silica microspheres have been successfully prepared, the existing methods generally have disadvantages such as complex synthesis steps and short phosphorescence lifetime, and usually require the synthesis of carbon dots first and then the encapsulation of carbon dots into monodisperse silica microspheres. In addition, since the complex surface chemical structure of carbon dots will destroy the condensation kinetics of tetraethyl orthosilicate, it is difficult to obtain uniform and monodisperse carbon dots@silica microspheres in this way, which seriously limits its further development and application. Therefore, it is very necessary to design and develop an in situ preparation method for obtaining long-lifetime room temperature phosphorescent carbon dots@silica microspheres with monodispersity. Summary of the invention

[0004] In order to avoid the shortcomings of the prior art, the present invention provides a monodisperse long-life room temperature phosphorescent carbon dot@silica microsphere and a preparation method thereof.

[0005] One of the purposes of the present invention is to provide a simple and easy in-situ preparation method.

[0006] The second object of the present invention is to provide a monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres.

[0007] The monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres prepared by the present invention are prepared by an in-situ synthesis method using glucose, polyvinyl pyrrolidone (PVP), ammonia water and tetraethyl orthosilicate (TEOS) as raw materials, and the preparation process includes the following specific steps: 1. First, add 0.2-0.8 g glucose, 0.1-1 g PVP and 2-8 mL ammonia water to a mixed solution of 7 mL ethanol and 2 mL water to obtain a transparent solution; 2. Add 1-5 mL TEOS to the transparent solution obtained in step 1 and stir for 6-24 hours to obtain a milky white solution; 3. Transfer the milky white solution obtained in step 2 to a polytetrafluoroethylene-lined reactor, and react at 160-200 °C for 6-24 hours to obtain a yellow-brown solution; 4. Centrifuge the yellow-brown solution obtained in step 3 at 8000 rpm for 5 minutes using a high-speed centrifuge, remove the supernatant in the centrifuge tube, and obtain a brown precipitate; 5. Dry the brown precipitate obtained in step 4 in an oven at 40-80°C for 12-36 hours to obtain a brown solid; 6. The brown solid obtained in step 5 is placed in a covered crucible and calcined in a muffle furnace at 500-600° C. for 2 hours to obtain monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres.

[0008] Beneficial effects of the present invention: 1. The present invention provides a monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres and a preparation method thereof, which is characterized in that glucose, PVP, ammonia water and TEOS are used as raw materials and prepared by an in-situ synthesis method, and only common laboratory equipment is required, and no special equipment is required, and the process is simple and easy to operate; 2. The monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres obtained by this method have a phosphorescence lifetime of 1.05 s. After turning off the UV light, the long-lifetime phosphorescence can be observed by the naked eye for 16 s. 3. The drugs used in the present invention are cheap and readily available, and the preparation process is simple and convenient, without complicated and tedious post-processing steps, and are particularly suitable for batch and low-cost preparation, and are suitable for industrial-scale production and commercial application; 4. The monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres provided by the present invention can be successfully applied in fields such as information encryption. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the embodiments or the description of the prior art will be briefly introduced with drawings below, but the drawings in the following description are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0010] Figure 1 This is a transmission electron microscope image of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1 of the present invention.

[0011] Figure 2 This is the X-ray diffraction pattern of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1 of the present invention.

[0012] Figure 3 This is a phosphorescence spectrum of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1 of the present invention.

[0013] Figure 4 This is a phosphorescence lifetime diagram of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1 of the present invention.

[0014] Figure 5 These are the state diagrams of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Examples 1-3 and Comparative Examples 1-2 under sunlight, under 365 nm ultraviolet light, and after the ultraviolet light is turned off.

[0015] Figure 6 This is a photo of the application of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1 of the present invention in information encryption. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0017] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0018] Unless otherwise specified, the experimental methods described in the following examples are all conventional methods; the reagents and materials described are all commercially available unless otherwise specified.

[0019] Embodiment 1: First, 0.5 g of glucose and 0.6 g of PVP were added to a mixed solution of 7 mL of ethanol and 2 mL of water, and 6 mL of ammonia and 3 mL of TEOS were added and stirred for 12 hours to obtain a milky white solution; the obtained solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 180°C for 12 hours to obtain a yellow-brown solution, which was centrifuged at 8000 rpm for 5 minutes in a high-speed centrifuge, and the supernatant in the centrifuge tube was removed to obtain a brown precipitate; the brown precipitate was dried in an oven at 80°C for 24 hours to obtain a brown solid; the brown solid was placed in a covered crucible and calcined at 550°C in a muffle furnace for 2 hours to obtain monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres.

[0020] Embodiment 2: First, 0.2 g of glucose and 1 g of PVP were added to a mixed solution of 7 mL of ethanol and 2 mL of water, and 8 mL of ammonia water and 5 mL of TEOS were added and stirred for 6 hours to obtain a milky white solution; the obtained solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 200 °C for 6 hours to obtain a yellow-brown solution, which was centrifuged at 8000 rpm for 5 minutes in a high-speed centrifuge, and the supernatant in the centrifuge tube was removed to obtain a brown precipitate; the brown precipitate was dried in a 40 °C oven for 36 hours to obtain a brown solid; the brown solid was placed in a covered crucible and calcined at 500 °C in a muffle furnace for 2 hours to obtain monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres.

[0021] Embodiment 3: First, 0.8 g of glucose and 0.1 g of PVP were added to a mixed solution of 7 mL of ethanol and 2 mL of water, and 2 mL of ammonia and 1 mL of TEOS were added and stirred for 24 hours to obtain a milky white solution; the obtained solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 160 °C for 24 hours to obtain a yellow-brown solution, which was centrifuged at 8000 rpm for 5 minutes in a high-speed centrifuge, and the supernatant in the centrifuge tube was removed to obtain a brown precipitate; the brown precipitate was dried in a 60 °C oven for 12 hours to obtain a brown solid; the brown solid was placed in a covered crucible and calcined at 600 °C in a muffle furnace for 2 hours to obtain monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres.

[0022] Comparative Example 1: First, 0.5 g of glucose was added to a mixed solution of 7 mL of ethanol and 2 mL of water, and stirred for 1 hour to obtain a transparent solution. The obtained transparent solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 180 °C for 12 hours to obtain a yellow-brown suspension; the obtained solution was centrifuged at 8000 rpm for 5 minutes using a high-speed centrifuge to separate the supernatant, and the supernatant was dialyzed in a 1000 Da dialysis bag for 48 hours to obtain a CDs solution. 1 mL of CDs solution, 0.6 g of PVP and 6 mL of ammonia water were added to 7 mL of ethanol solution, and 3 mL of TEOS was added under stirring. The stirring was continued for 12 hours to obtain a milky white solution. The milky white solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 180 °C for 12 hours to obtain a yellow-brown solution. The solution was centrifuged at 8000 rpm for 5 minutes in a high-speed centrifuge, and the supernatant in the centrifuge tube was removed to obtain a brown precipitate. The brown precipitate was dried in an oven at 80 °C for 24 hours to obtain a brown solid. The brown solid was placed in a covered crucible and calcined at 550 °C in a muffle furnace for 2 hours to obtain monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres.

[0023] Comparative Example 2: First, 6 mL of ammonia water was added to a mixed solution of 7 mL of ethanol and 2 mL of water, and then 3 mL of TEOS was added and stirred for 12 hours to obtain a milky white solution; the obtained solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 180°C for 12 hours to obtain a milky white solution, which was centrifuged at 8000 rpm for 5 minutes in a high-speed centrifuge, and the supernatant in the centrifuge tube was removed to obtain a white precipitate; the white precipitate was dried in an oven at 80°C for 24 hours to obtain silica. 0.1 g silica, 0.5 g glucose and 0.6 g PVP were added to a mixed solution of 7 mL ethanol and 2 mL water and stirred for 12 hours to obtain a milky white solution. The milky white solution was transferred to a polytetrafluoroethylene-lined reactor and reacted at 180 °C for 12 hours to obtain a yellow-brown solution. The solution was centrifuged at 8000 rpm for 5 minutes in a high-speed centrifuge, and the supernatant in the centrifuge tube was removed to obtain a brown precipitate. The brown precipitate was dried in an oven at 80 °C for 24 hours to obtain a brown solid. The brown solid was placed in a covered crucible and calcined at 550 °C in a muffle furnace for 2 hours to obtain monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres.

[0024] Figure 1 This is a transmission electron microscope image of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1. Figure 1 It can be seen that the average diameter of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres is about 300 nm, and the sample has very good dispersibility.

[0025] Figure 2 This is the X-ray diffraction image of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1. Figure 2 It can be seen that the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres exhibit an amorphous structure.

[0026] Figure 3 This is the phosphorescence spectrum of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1. Figure 3 It can be seen that when the excitation wavelength is 365 nm, the center of its phosphorescence emission band is located around 550 nm.

[0027] Figure 4 This is the phosphorescence lifetime diagram of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1. Figure 4 It can be seen that the time-resolved decay spectrum is fitted using a three-exponential function according to the following formula: τ avg =∑α i τ i 2 / ∑α i τ i The average phosphorescence lifetime at room temperature was calculated to be 1.05 s, indicating that the prepared monodisperse long-lifetime room-temperature phosphorescent carbon dots@silica microspheres have an excellent long phosphorescence lifetime.

[0028] Figure 5 The state diagrams of the monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres prepared in Examples 1-3 and Comparative Examples 1-2 under sunlight, under 365 nm ultraviolet light, and after turning off the light. Figure 5 It can be seen that Example 1 exhibits the longest visible phosphorescence duration of 16 s; the phosphorescence visible to the naked eye time of the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres prepared in other Examples 2-3 and Comparative Examples 1-2 is relatively short.

[0029] Figure 6 This is a photo of the application of the monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres prepared in Example 1 in information encryption. As shown in the figure, it is an information encryption model designed in combination with binary code, and three colors of samples are used to represent different information, for example: yellow represents "10", green represents "0", and blue represents "1". Under 365 nm ultraviolet light, the samples all show blue fluorescence but cannot distinguish valid information. After the ultraviolet light is turned off, due to the different phosphorescent colors of the samples, the information "UJN" can be accurately deciphered according to different colors.

[0030] Obviously, those skilled in the art can make various changes and modifications to the monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres and the preparation method thereof described in the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres, comprising the following steps: First, 0.2-0.8 g of glucose and 0.1-1 g of PVP are added to a mixed solution of 7 mL of ethanol and 2 mL of water, and 2-8 mL of ammonia water is added to obtain a transparent solution; then 1-5 mL of TEOS is added, and stirring is continued for 6-24 hours to obtain a milky white solution; the obtained solution is transferred to a polytetrafluoroethylene-lined reactor, and reacted at 160-200°C for 6-24 hours. The reacted solution is centrifuged at 8000 rpm for 5 minutes in a high-speed centrifuge, and the upper clear liquid in the centrifuge tube is removed to obtain a brown precipitate; the precipitate is placed in a 40-80°C oven and dried for 12-36 hours to obtain a brown solid; the precipitate is placed in a covered crucible and calcined at 500-600°C in a muffle furnace for 2 hours to obtain a monodisperse long-lifetime room temperature phosphorescent carbon dot@silica microsphere.

2. The method for preparing monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres according to claim 1, characterized in that: The amount of glucose used was 0.5 g, and the amount of PVP used was 0.6 g.

3. The method for preparing monodisperse long-lifetime room temperature phosphorescent carbon dots@silica microspheres according to claim 1, characterized in that: The amount of ammonia water used was 6 mL, and the amount of TEOS used was 3 mL.

4. The use of monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres prepared by the preparation method according to claim 1, characterized in that: The monodisperse long-life room temperature phosphorescent carbon dots@silica microspheres are applied to information encryption.

Citation Information

Patent Citations

  • SiO2 / carbon dot hybrid nano material as well as preparation method and application thereof

    CN115216293A

  • Room-temperature phosphorescent carbon dot and allophane composite material and preparation method thereof

    CN116590007A

  • Sunlight-excited room-temperature phosphorescent carbon dot-alumina composite material and preparation method thereof

    CN117903795A

  • Long-service-life room-temperature phosphorescent carbon-dot-loaded silicon dioxide sphere as well as controllable preparation method and application thereof

    CN118256229A

  • Nanocarbon-iron composite system, composition, preparation method, and application thereof

    WO2018137708A1

Cited By

  • Long-afterglow silicon dioxide nanoparticles as well as preparation method and application thereof

    CN120793934A

  • A low-temperature preparation method of an alkali-resistant room-temperature phosphorescent carbon dot composite material in a confined state and application thereof

    CN122878952A