Method for preparing superfine aluminum hydroxide from sodium chromate carbonized by-product

The method of preparing ultra-fine aluminum hydroxide through sodium chromate carbonization by-product solves the problems of complex process and high cost in the existing technology, realizes the preparation of high-purity, ultra-fine-grained aluminum hydroxide, and utilizes the by-product for resource development Recycling improves product stability and hydrophobicity.

CN118724035APending Publication Date: 2024-10-01SICHUAN YINHE CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410879320.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing preparation method of ultrafine aluminum hydroxide, the raw materials mainly rely on industrial-grade aluminum hydroxide. The process is complex and costly, and aluminum-containing resources cannot be effectively utilized, resulting in the particle size and purity of aluminum hydroxide failing to meet actual needs.

Method used

A method for preparing ultrafine aluminum hydroxide from sodium chromate carbonization by-products, including passing carbon dioxide into a sodium chromate solution to generate sodium bicarbonate, controlling the pH value to precipitate aluminum into ultrafine aluminum hydroxide, and converting hexafluoride into hydrazine hydrate. The valent chromium is trivalent chromium ion, which is then washed, filtered and air-dried. Finally, it is modified with methyl silicone oil and ball milled to reduce the particle size and improve stability.

Benefits of technology

The preparation of high-purity, ultra-fine-grained aluminum hydroxide is achieved, with excellent filtration performance. The by-product can be recycled in chromium salt production, reducing production costs, and improving the stability and hydrophobicity of aluminum hydroxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724035A_ABST
    Figure CN118724035A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing superfine aluminum hydroxide from sodium chromate carbonized by-products, which comprises the following steps: introducing carbon dioxide into a sodium chromate solution, and performing solid-liquid separation after reaction to obtain a sodium bicarbonate solid; adding a sodium bicarbonate solid into the aluminum-containing sodium chromate alkali liquor to control the pH value of the aluminum-containing sodium chromate alkali liquor, reacting to obtain superfine aluminum hydroxide, washing and filtering the superfine aluminum hydroxide to obtain low-sodium superfine aluminum hydroxide, adding hydrazine hydrate into the low-sodium superfine aluminum hydroxide, and pulping for deep purification treatment; and washing and filtering the pulped and purified low-sodium superfine aluminum hydroxide again, and then carrying out airflow drying to prepare the pure superfine aluminum hydroxide. The method has the beneficial effects that superfine aluminum hydroxide generated under a carbonic acid system has excellent filtering performance and can be comparable with aluminum hydroxide prepared by a seed precipitation method; the finished product can be obtained by airflow drying without evaporating the solution like a seed precipitation method; the methyl silicone oil is used for modifying the aluminum hydroxide powder, so that the aluminum hydroxide powder has better stability and hydrophobicity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparing aluminum hydroxide, and more specifically, the invention relates to a method for preparing ultrafine aluminum hydroxide from a byproduct of sodium chromate carbonization. Background Art

[0002] Ultrafine aluminum hydroxide is currently mainly used as a flame retardant filler in materials such as wires and cables, insulators, and in photovoltaic new energy materials such as photovoltaic adhesives and lithium battery separators. At present, the many methods for preparing ultrafine aluminum hydroxide can be mainly divided into physical and chemical methods. Chemical methods include microemulsion method, metal alkoxide method, supergravity method, solid phase method, sodium aluminate solution carbon fractionation method, seed decomposition method, etc. However, the raw materials in the existing methods mainly focus on ready-made chemicals, and there is a lack of research on the comprehensive utilization of aluminum-containing resources. In the production of chromium salts, chromite naturally contains aluminum, which is an impurity for chromium salt products and needs to be removed. Therefore, ultrafine aluminum hydroxide is prepared while ensuring the quality of chromium salt products to achieve high-value utilization of aluminum resources.

[0003] Patent CN116143152A discloses an ultrafine aluminum hydroxide and its preparation method and application, and ultrafine aluminum hydroxide is prepared by controlling the caustic ratio of the seed separation semen, the dissolution temperature and the seed separation temperature during the preparation process. The raw material of this method is industrial-grade aluminum hydroxide, and the process flow is long, the process is complex, and the industrial production cost is high.

[0004] The particle size and purity of the aluminum hydroxide produced in the above prior art still cannot meet the demand for ultrafine high-purity aluminum hydroxide in actual use. Summary of the invention

[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0006] In order to achieve these purposes and other advantages according to the present invention, a method for preparing ultrafine aluminum hydroxide from a byproduct of sodium chromate carbonization is provided, comprising the following steps:

[0007] Step 1, introducing carbon dioxide into the sodium chromate solution, and separating the solid and the liquid after the reaction to obtain sodium bicarbonate solid;

[0008] Step 2: adding the sodium bicarbonate solid obtained in step 1 to the sodium chromate-containing alkali solution to control the pH of the sodium chromate-containing alkali solution, and after the reaction, aluminum in the solution is precipitated in the form of ultrafine aluminum hydroxide to obtain by-products of sodium carbonate and sodium bicarbonate;

[0009] Step 3: Wash and filter the ultrafine aluminum hydroxide obtained in step 2 to obtain low-sodium ultrafine aluminum hydroxide, then add hydrazine hydrate to the low-sodium ultrafine aluminum hydroxide, and perform pulping and purification to convert hexavalent chromium impurities in the low-sodium ultrafine aluminum hydroxide into trivalent chromium ions;

[0010] Step 4: Filter and wash the low sodium ultrafine aluminum hydroxide purified by pulping in step 3 again, and then air dry it to obtain pure ultrafine aluminum hydroxide.

[0011] Preferably, in step 1, the chromium element in the sodium chromate solution is less than 10 wt % in terms of Cr2O3, the carbon dioxide is industrial grade, and the reaction temperature is controlled at 25°C to 45°C.

[0012] Preferably, in the step 2, the Al2O3 content in the sodium aluminum chromate alkali solution is 1wt% to 10wt%, the sodium ion concentration is 50g / L to 120g / L, the pH is controlled to be 9.5 to 10.5 by the addition amount of sodium bicarbonate, and the reaction temperature is controlled to be 15°C to 40°C.

[0013] Preferably, in step 1, the volume flow ratio of carbon dioxide to sodium chromate solution is 1-2 L / min:1 L / min.

[0014] Preferably, in the step 2, the byproducts sodium carbonate and sodium bicarbonate obtained are returned to the sodium chromate solution in the step 1 for recycling.

[0015] Preferably, in the step three, the molar ratio of hydrazine hydrate to hexavalent chromium in the low-sodium ultrafine aluminum hydroxide is 1:1 to 2.5.

[0016] Preferably, in the step three, ultrapure water is first added to the mixture of low sodium ultrafine aluminum hydroxide and hydrazine hydrate at a solid-liquid ratio of 1:1 during slurrying, and slurrying is performed after stirring evenly, and the slurrying time is 60 minutes.

[0017] Preferably, in step three, the pH of the solution is maintained at 7 to 7.8 after slurrying.

[0018] Preferably, the Cr content in the pure ultrafine aluminum hydroxide prepared in step 4 is 6+ ≤0.001%,Na + ≤0.0008%.

[0019] Preferably, the particle size D50 of the pure ultrafine aluminum hydroxide obtained in step 4 is 0.6 μm to 1.2 μm.

[0020] Preferably, the purified ultrafine aluminum hydroxide obtained in step 4 is post-treated by the following steps:

[0021] S1. Dissolve methyl silicone oil in kerosene, stir evenly, and prepare a methyl silicone oil modified solution, wherein the mass ratio of methyl silicone oil to kerosene is 1:6-12;

[0022] S2, adding pure ultrafine aluminum hydroxide to a ball mill, heating and ball milling, the heating temperature is 30-65°C, the ball milling speed is 600-800rpm, and the ball milling is 30-60min. During the ball milling process, the methyl silicone oil modified solution obtained in S1 is added to the ball mill in the form of high-pressure spray, wherein the mass ratio of pure ultrafine aluminum hydroxide to the methyl silicone oil modified solution is 10:0.05-2;

[0023] S3. Add 5wt% tetramethylammonium hydroxide solution to the ball mill and continue ball milling for 5-15 minutes. After ball milling, vacuum dry at 70-110°C for 2-10 hours and then transfer to a jet mill to break up to obtain modified ultrafine aluminum hydroxide, wherein the mass ratio of the methyl silicone oil modified solution to 5wt% tetramethylammonium hydroxide is 4:1-2, and the vacuum degree of vacuum drying is 0.02-10Pa.

[0024] The present invention has at least the following beneficial effects:

[0025] (1) The ultrafine aluminum hydroxide produced in the carbonate (Na2CO3, NaHCO3) system is sandy and has excellent filtration performance. Other ultrafine aluminum hydroxide Cr after washing 6+ ≤0.001%,Na + ≤0.0008%, comparable to aluminum hydroxide produced by seed separation method;

[0026] (2) This method does not require evaporation of the solution like the seed separation method, and the finished product can be obtained by air drying;

[0027] (3) The byproducts and chromium-containing wastes generated during the process can be used in the subsequent production of chromium salts, thus realizing the recycling of resources, which is economical and environmentally friendly;

[0028] (4) The surface of aluminum hydroxide powder is modified by using methyl silicone oil. After the methyl silicone oil is attached to the surface of the aluminum hydroxide powder, the methyl silicone oil molecules are tightly coated on the surface of the aluminum hydroxide powder through a catalyst, so that the aluminum hydroxide powder has better stability and hydrophobicity. At the same time, the particle size of the aluminum hydroxide powder is further reduced by ball milling.

[0029] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic diagram of the method flow of Example 1 of the present invention. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0032] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0033] It should be noted that in the description of the present invention, the orientation or positional relationship indicated by the term is based on the orientation or positional relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0034] Example 1

[0035] like Figure 1 As shown, a method for preparing ultrafine aluminum hydroxide from a byproduct of sodium chromate carbonization of the present invention comprises the following steps:

[0036] Step 1, introducing industrial grade carbon dioxide into a sodium chromate solution with a concentration of 9.5wt% (in terms of Cr2O3), the gas-liquid volume flow ratio of carbon dioxide to the sodium chromate solution is 2L / min:1L / min, the reaction temperature is 20°C, and after the reaction, solid-liquid separation is performed to obtain sodium bicarbonate solid for standby use;

[0037] Step 2: Add the sodium bicarbonate obtained in step 1 to 100L of sodium chromate-containing alkali solution (sodium ion concentration of 76g / L, aluminum content of 5.3wt% in terms of Al2O3) until the pH of the sodium chromate-containing alkali solution is 9.5, and the reaction temperature is 28°C. After the reaction, aluminum in the solution is precipitated in the form of ultrafine aluminum hydroxide, and the by-products sodium carbonate and sodium bicarbonate are returned to step 1 (returning the by-products to step 1 is helpful to produce sodium bicarbonate);

[0038] Step 3: Wash and filter the ultrafine aluminum hydroxide obtained in step 2 with pure water to obtain low-sodium ultrafine aluminum hydroxide, add hydrazine hydrate to the low-sodium ultrafine aluminum hydroxide, and then add ultrapure water to the mixture of low-sodium ultrafine aluminum hydroxide and hydrazine hydrate at a solid-liquid ratio of 1:1, stir evenly and then beat, perform deep purification, the beating time is 60 minutes, and the pH is maintained at 7.5 after beating. Cr in low-sodium ultrafine aluminum hydroxide 6+ Converted to Cr 3+ ; The molar ratio of hydrazine hydrate to hexavalent chromium in low-sodium ultrafine aluminum hydroxide is 1:2;

[0039] Step 4: Wash and filter the low-sodium ultrafine aluminum hydroxide purified by pulping in step 3 again with pure water, and then air dry it to obtain pure ultrafine aluminum hydroxide.

[0040] The particle size D50 of the pure ultrafine aluminum hydroxide prepared in this embodiment is 0.82 μm, and the Cr 6+ The content is 0.0008%, Na + The content is 0.0005% and the purity of aluminum hydroxide reaches 99.993%.

[0041] Example 2

[0042] A method for preparing ultrafine aluminum hydroxide from a byproduct of sodium chromate carbonization comprises the following steps:

[0043] Step 1, introducing industrial grade carbon dioxide into a sodium chromate solution with a concentration of 9.5wt% (in terms of Cr2O3), with the gas-liquid volume flow ratio of carbon dioxide to the sodium chromate solution being 1.5L / min:1L / min, and separating the solid and the liquid after the reaction to obtain sodium bicarbonate solid for standby use;

[0044] Step 2: Add the sodium bicarbonate obtained in step 1 to 100L of sodium chromate-containing alkali solution (sodium ion concentration is 76g / L, aluminum content is 4.6wt% in terms of Al2O3), control the pH of the sodium chromate-containing alkali solution to be 10.0, and the reaction temperature to be 25°C. After the reaction, aluminum in the solution is precipitated in the form of ultrafine aluminum hydroxide, and the by-products sodium carbonate and sodium bicarbonate are returned to step 1 (returning the by-products to step 1 is helpful to produce sodium bicarbonate);

[0045] Step 3: Wash and filter the ultrafine aluminum hydroxide obtained in step 2 with pure water to obtain low-sodium ultrafine aluminum hydroxide, add hydrazine hydrate to the low-sodium ultrafine aluminum hydroxide, and then add ultrapure water to the mixture of low-sodium ultrafine aluminum hydroxide and hydrazine hydrate at a solid-liquid ratio of 1:1, stir evenly and then beat, perform deep purification, the beating time is 60 minutes, and the pH is maintained at 7.8 after beating, and Cr in the low-sodium ultrafine aluminum hydroxide is removed. 6+ Converted to Cr 3+ , wherein the molar ratio of hydrazine hydrate to hexavalent chromium in low-sodium ultrafine aluminum hydroxide is 1:2.5;

[0046] Step 4: Wash and filter the low-sodium ultrafine aluminum hydroxide purified by pulping in step 3 again with pure water, and then air dry it to obtain pure ultrafine aluminum hydroxide.

[0047] The particle size D50 of the pure ultrafine aluminum hydroxide prepared in this embodiment is 0.78 μm, and the Cr 6+ The content is 0.0007%, Na + The content is 0.0006% and the purity of aluminum hydroxide reaches 99.991%.

[0048] Example 3

[0049] A method for preparing ultrafine aluminum hydroxide from a byproduct of sodium chromate carbonization comprises the following steps:

[0050] Step 1, introducing industrial grade carbon dioxide into a sodium chromate solution with a concentration of 9.5wt% (in terms of Cr2O3), with the gas-liquid volume flow ratio of carbon dioxide to the sodium chromate solution being 1L / min:1L / min, and separating the solid and the liquid after the reaction to obtain sodium bicarbonate solid for standby use;

[0051] Step 2: Add the sodium bicarbonate obtained in step 1 to 100L of sodium chromate-containing alkali solution (sodium ion concentration is 71g / L, aluminum content is 6.4wt% in terms of Al2O3), control the pH of the sodium chromate-containing alkali solution to be 10.0, and the reaction temperature to be 20°C. After the reaction, aluminum in the solution is precipitated in the form of ultrafine aluminum hydroxide, and the by-products sodium carbonate and sodium bicarbonate are returned to step 1 (returning the by-products to step 1 is helpful to produce sodium bicarbonate);

[0052] Step 3: Wash and filter the ultrafine aluminum hydroxide obtained in step 2 with pure water to obtain low-sodium ultrafine aluminum hydroxide, add hydrazine hydrate to the low-sodium ultrafine aluminum hydroxide, and then add ultrapure water to the mixture of low-sodium ultrafine aluminum hydroxide and hydrazine hydrate at a solid-liquid ratio of 1:1, stir evenly and then beat, perform deep purification, the beating time is 60 minutes, and the pH is maintained at 7.8 after beating, and Cr in the low-sodium ultrafine aluminum hydroxide is removed. 6+ Converted to Cr 3+ , wherein the molar ratio of hydrazine hydrate to hexavalent chromium in low-sodium ultrafine aluminum hydroxide is 1:1.5;

[0053] Step 4: Wash and filter the low-sodium ultrafine aluminum hydroxide purified by pulping in step 3 again with pure water, and then air dry it to obtain pure ultrafine aluminum hydroxide.

[0054] The particle size D50 of the pure ultrafine aluminum hydroxide prepared in this embodiment is 0.75 μm, and the Cr 6+ The content is 0.0009%, Na + The content is 0.0005% and the purity of aluminum hydroxide reaches 99.996%.

[0055] Example 4

[0056] The difference between this embodiment and embodiment 3 is that the purified ultrafine aluminum hydroxide obtained in step 4 is post-treated, comprising the following steps:

[0057] S1. Dissolve 4 g of methyl silicone oil in 32 g of kerosene and stir evenly to prepare a methyl silicone oil modified solution;

[0058] S2, add 360g of pure ultrafine aluminum hydroxide into a ball mill, heat to 45°C, and perform ball milling at a speed of 600rpm for 40min. During the ball milling process, add the methyl silicone oil modified solution obtained in S1 into the ball mill by high-pressure spraying;

[0059] S3. Add 9 g of 5 wt% tetramethylammonium hydroxide solution into the ball mill and continue ball milling for 10 min. After ball milling, dry the mixture in vacuum at 80° C. and 5 Pa for 3 h, then transfer the mixture to a jet mill to break it up, thereby obtaining modified ultrafine aluminum hydroxide.

[0060] The modified ultrafine aluminum hydroxide prepared in this embodiment has a particle size D50 of 0.4 μm, a contact angle of 138°, and good hydrophobicity.

[0061] Example 5

[0062] The difference between this embodiment and embodiment 3 is that the purified ultrafine aluminum hydroxide obtained in step 4 is post-treated, comprising the following steps:

[0063] S1. Dissolve 6 g of methyl silicone oil in 36 g of kerosene and stir evenly to prepare a methyl silicone oil modified solution;

[0064] S2, add 420g of pure ultrafine aluminum hydroxide into a ball mill, heat to 45°C, and perform ball milling at a speed of 600rpm for 40min. During the ball milling process, add the methyl silicone oil modified solution obtained in S1 into the ball mill by high-pressure spraying;

[0065] S3. Add 10.5 g of 5 wt% tetramethylammonium hydroxide solution into the ball mill and continue ball milling for 10 min. After ball milling, dry the mixture in vacuum at 80° C. and 5 Pa for 3 h, then transfer the mixture to a jet mill to break it up, thereby obtaining modified ultrafine aluminum hydroxide.

[0066] The modified ultrafine aluminum hydroxide prepared in this embodiment has a particle size D50 of 0.36 μm, a contact angle of 143°, and good hydrophobicity.

[0067] Comparative Example 1

[0068] The difference between this comparative example and Example 4 is that in S2, no ball milling is performed, but stirring and heating are used. The rest is consistent with Example 4. The particle size d50 of the modified ultrafine aluminum hydroxide finally obtained is 0.76 μm, the contact angle is 120°, and the hydrophobic property is average.

[0069] Comparative Example 2

[0070] The difference between this comparative example and Example 4 is that methyl silicone oil is not used to modify the aluminum hydroxide powder, but the aluminum hydroxide powder is directly ball-milled. The particle size D50 of the modified ultrafine aluminum hydroxide finally obtained is 0.4 μm, the contact angle is only 86°, and the hydrophobic performance is poor.

[0071] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for preparing ultrafine aluminum hydroxide from the byproduct of sodium chromate carbonization, characterized in that: The following steps are involved: Step 1, introducing carbon dioxide into the sodium chromate solution, and separating the solid and the liquid after the reaction to obtain sodium bicarbonate solid; Step 2: adding the sodium bicarbonate solid obtained in step 1 to the sodium chromate-containing alkali solution to control the pH of the sodium chromate-containing alkali solution, and after the reaction, aluminum in the solution is precipitated in the form of ultrafine aluminum hydroxide to obtain by-products of sodium carbonate and sodium bicarbonate; Step 3: Wash and filter the ultrafine aluminum hydroxide obtained in step 2 to obtain low-sodium ultrafine aluminum hydroxide, then add hydrazine hydrate to the low-sodium ultrafine aluminum hydroxide, and perform pulping and purification to convert hexavalent chromium impurities in the low-sodium ultrafine aluminum hydroxide into trivalent chromium ions; Step 4: Filter and wash the low sodium ultrafine aluminum hydroxide purified by pulping in step 3 again, and then air dry it to obtain pure ultrafine aluminum hydroxide.

2. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: In the step 1, the chromium element in the sodium chromate solution is less than 10wt% in terms of Cr2O3, the carbon dioxide is industrial grade, and the reaction temperature is controlled at 25°C to 45°C.

3. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: In the step 1, the volume flow ratio of carbon dioxide to sodium chromate solution is 1-2 L / min:1 L / min.

4. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: In the step 2, the Al2O3 content in the sodium aluminum chromate alkali solution is 1wt% to 10wt%, the sodium ion concentration is 50g / L to 120g / L, the pH is controlled to be 9.5 to 10.5 by the addition amount of sodium bicarbonate, and the reaction temperature is controlled to be 15°C to 40°C.

5. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: In the step 2, the byproducts sodium carbonate and sodium bicarbonate obtained are returned to the sodium chromate solution in the step 1 for recycling.

6. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: In the step 3, the molar ratio of hydrazine hydrate to hexavalent chromium impurities in the low-sodium ultrafine aluminum hydroxide is 1:1 to 2.

5.

7. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: In the step three, when beating, ultrapure water is first added to the mixture of low-sodium ultrafine aluminum hydroxide and hydrazine hydrate at a solid-liquid ratio of 1:1, and the mixture is evenly stirred before beating. The beating time is 60 minutes.

8. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: In the step 3, the pH of the solution is maintained at 7 to 7.8 after pulping.

9. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: The Cr content in the pure ultrafine aluminum hydroxide prepared in step 4 is 6+ ≤0.001%,Na + ≤0.0008%.

10. The method for preparing ultrafine aluminum hydroxide from the carbonization byproduct of sodium chromate according to claim 1, characterized in that: The particle size D50 of the pure ultrafine aluminum hydroxide obtained in step 4 is 0.6 μm to 1.2 μm.