Coal gangue resourceful treatment method and system
Through the activation treatment and acid leaching reaction of coal gangue, combined with the ammonium sulfate crystallization treatment, the efficient resource utilization of aluminum and silicon in coal gangue is achieved, which solves the problems of low resource utilization rate and complicated process in the existing technology, and obtains High-purity silica micropowder and aluminum ammonium sulfate simplify the process and reduce environmental impact.
Patent Information
- Application Number
- CN202410883522.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology cannot effectively improve the resource utilization rate of coal gangue. The process is complex and the purity is low, making it impossible to achieve efficient resource utilization of coal gangue.
By activating coal gangue at 200°C to 800°C, it is transformed into amorphous metakaolinite, and is subjected to an acid leaching reaction with sulfuric acid solution, and then mixed with ammonium sulfate for crystallization treatment, and the sulfuric acid solution is recycled to achieve Efficient extraction of aluminum and silicon.
It achieves efficient resource utilization of aluminum and silicon in coal gangue, simplifies the process steps, increases the leaching rate of aluminum, reduces the sulfuric acid concentration and temperature requirements for the acid leaching reaction, avoids secondary pollution, and obtains silicon micropowder and sulfuric acid. Aluminum ammonium has high purity and is suitable for industrial and food applications.
Smart Images

Figure CN118724042A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste treatment, and specifically relates to a method and system for treating coal gangue resources. Background Art
[0002] Energy is a necessity for the survival and development of human society. Coal, as an important type of energy, is still the main energy source for human beings, accounting for 77% and more than 70% of the total primary energy production and consumption, respectively. For a long time, the energy structure dominated by coal will not change significantly. However, mining 1 ton of coal can produce 0.25 to 0.33 tons of coal gangue, resulting in a large amount of coal gangue stockpiling, which not only occupies land, but also causes great harm to the ecological environment.
[0003] At present, the utilization of coal gangue has been expanded from paving roads and concrete admixtures to brick making, cement and other aspects. However, there are a lot of high-aluminum coal gangue in some areas. If it is only used for paving roads, concrete, brick making, cement and other aspects, the resource utilization rate is too low. If it is upgraded to mineral resources and the aluminum and silicon in it are effectively extracted, the utilization value of coal gangue will be greatly improved.
[0004] In the prior art, there are methods for extracting mineral resources from waste slag, such as processing high-aluminum, high-silicon and high-iron ores to obtain silicon dioxide and ammonium aluminum sulfate, and processing titanium ore to obtain silicon dioxide and ammonium aluminum sulfate. However, these treatment methods in the prior art are either too complicated, such as requiring too many acid leaching times and complex reaction conditions for extracting aluminum, or the purity of the extracted silicon dioxide and ammonium aluminum sulfate is low, and the components in these waste slags are greatly different from those in coal gangue. These existing treatment methods cannot achieve high resource utilization of coal gangue. Summary of the invention
[0005] Based on the above situation, the main purpose of the present invention is to provide a method and system for resource processing of coal gangue, so as to achieve efficient resource utilization of coal gangue, and the process is simple and can be widely used in industrial processing.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] The first aspect of the present invention provides a method for recycling coal gangue, wherein the coal gangue includes silicon, aluminum and a burnt-out component, the sum of the oxide contents of silicon and aluminum is greater than or equal to 70%, and the burnt-out component includes a carbonaceous component and organic matter; the method comprises the following steps:
[0008] S10: grinding the gangue, and performing activation treatment at 200° C. to 800° C. to obtain an activated sample, wherein the burn-out component is burned out during the activation treatment, and the carbonaceous component provides heat for the activation process; the obtained activated sample includes silicon and aluminum, and the silicon and aluminum mainly exist in the form of amorphous metakaolinite;
[0009] S20: subjecting the activated sample to an acid leaching reaction with a sulfuric acid solution having a concentration of 1 to 9 mol / L at a liquid-to-solid ratio of 4 to 10, filtering to obtain a first filtrate and silicon powder, wherein the aluminum element enters the first filtrate; wherein the temperature of the reaction system is 40° C. to 100° C.;
[0010] S30: mixing the first filtrate with ammonium sulfate in a ratio of ammonia to aluminum of 1:1, performing crystallization after the reaction, and filtering to obtain a second filtrate and ammonium aluminum sulfate;
[0011] S40: After adjusting the second filtrate to the sulfuric acid concentration in step S20, return to step S20.
[0012] Optionally, in the step S10, the gangue is ground to a particle size less than or equal to 74 μm; and the activation treatment time is 30 min to 60 min.
[0013] Optionally, in step S20, the concentration of the sulfuric acid solution is 1 mol to 5 mol, and the sulfuric acid solution and the activated sample are stirred and dissolved for 10 min to 80 min and then filtered.
[0014] Optionally, in step S20, the total amount of sulfuric acid is controlled according to the sulfuric acid concentration and the liquid-solid ratio, wherein the sulfuric acid concentration is negatively correlated with the liquid-solid ratio.
[0015] Optionally, in step S20,
[0016] When the concentration of the sulfuric acid solution is 1 mol to 2 mol / L, the liquid-to-solid ratio is 6 to 10;
[0017] When the concentration of the sulfuric acid solution is 4 mol to 5 mol / L, the liquid-to-solid ratio is 4 to 5.
[0018] Optionally, in step S20, the concentration of the sulfuric acid is 2 mol / L; the liquid-to-solid ratio of the sulfuric acid solution to the activated sample is 6; and the temperature of the reaction system is 95°C.
[0019] Optionally, in step S30, the first filtrate is placed in a water bath at 40° C. to 100° C., ammonium sulfate is added thereto, stirred to dissolve the ammonium sulfate, and then cooled for crystallization.
[0020] Optionally, in step S30, the solution after the reaction is allowed to stand at room temperature for 0.5 h to 3 h, and then filtered to obtain ammonium aluminum sulfate crystals.
[0021] Optionally, after the step S40 is cycled for a preset number of times, the ammonium aluminum sulfate crystals obtained in the step S30 are recrystallized 1 to 2 times to obtain a finished ammonium aluminum sulfate product.
[0022] The second aspect of the present invention provides a gangue resource utilization system, which is used to implement the gangue resource processing method according to any one of the above claims; comprising:
[0023] A grinding device for grinding in step S10, an activation device for activation treatment in step S10, a mixing reaction device for acid leaching reaction in step S20 and reaction in step S30, and a filtering and separation device for filtering in steps S20 and S30.
[0024] The method for resource-based treatment of coal gangue provided by the present invention has the following advantages: first, no waste is generated or discharged during the entire process, the comprehensive utilization rate of the main elements aluminum and silicon in the coal gangue is high, and the obtained elements or mixtures can be used as raw materials in industrial production, which can produce good economic benefits, truly realize comprehensive and highly resource-based treatment of coal gangue, and greatly improve the overall utilization value of coal gangue; and there is no secondary waste discharge in the entire process, which is environmentally friendly and realizes the harmless treatment of coal gangue.
[0025] Secondly, by first activating the gangue, the reactivity of its mineral components can be changed. The high-content silicon-aluminum components will be transformed into amorphous kaolinite during the activation process, so that the subsequent acid leaching reaction only needs to be carried out once to achieve an aluminum leaching rate of more than 95%, or even more than 99%; and the requirements for sulfuric acid concentration and reaction system temperature in the acid leaching reaction can be reduced, thereby making the process simpler. At the same time, through the activation treatment, even the organic matter of the burnt-out components in the gangue can be burned off, thereby avoiding its entry into the subsequent acid leaching reaction and causing adverse effects on the reaction, and it can also make full use of the carbonaceous components in the burnt-out to provide a certain amount of heat energy in the activation treatment, thereby saving the requirements for heat energy in the reaction.
[0026] Thirdly, high-purity silicon micropowder can be obtained by filtering after the acid leaching reaction, and the first filtrate obtained by acid leaching can obtain high-purity ammonium aluminum sulfate after reacting with ammonium sulfate and crystallizing, which can be directly used in the food field, water treatment field, etc., and the second filtrate after extracting ammonium aluminum sulfate can also be recycled. It can be seen that the resource treatment method of coal gangue of the present invention can realize the full resource utilization of aluminum and silicon in coal gangue; and only one acid leaching process is required in the process of aluminum extraction, which greatly simplifies the entire aluminum extraction process steps, and can save resources without causing secondary pollution.
[0027] Other beneficial effects of the present invention will be explained in the specific implementation manner through the introduction of specific technical features and technical solutions. Through the introduction of these technical features and technical solutions, those skilled in the art should be able to understand the beneficial technical effects brought about by the technical features and technical solutions. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings.
[0029] Figure 1 A schematic flow chart of an implementation method of the resource processing method of coal gangue provided by the present invention;
[0030] Figure 2 This is a schematic diagram of the changes in components in each step in one implementation of the method for resource processing of coal gangue provided by the present invention. DETAILED DESCRIPTION
[0031] The present invention is described below based on embodiments, but the present invention is not limited to these embodiments. In the following detailed description of the present invention, some specific details are described in detail. In order to avoid confusing the essence of the present invention, known methods, processes, procedures, and components are not described in detail.
[0032] In addition, persons of ordinary skill in the art will appreciate that the drawings provided herein are for illustration purposes and are not necessarily drawn to scale.
[0033] Unless the context clearly requires otherwise, throughout the specification and claims, the words "include", "comprising" and similar words should be interpreted in an inclusive sense rather than an exclusive or exhaustive sense; that is, in the sense of "including but not limited to".
[0034] In the description of the present invention, it should be understood that the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. In addition, in the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0035] In the description of the present invention, "content" refers to mass percentage.
[0036] The present invention provides a method for processing coal gangue resources, which can be used to process coal gangue waste produced in coal mining, especially to effectively utilize coal gangue containing high aluminum silicon. Specifically, the coal gangue includes silicon, aluminum and burnt-out components, wherein the sum of the oxide contents of silicon and aluminum is greater than or equal to 70%. Specifically, the silicon element mainly exists in the form of silicon dioxide, and the aluminum element mainly exists in the form of aluminum oxide. Therefore, it can be said that the sum of the masses of silicon dioxide and aluminum oxide accounts for more than 70% of the total mass of the coal gangue, such as the sum of the oxide contents of silicon and aluminum is 70%, 72%, 75%, 77% or 80%, etc. Of course, the contents of silicon and aluminum oxides are not limited to the percentages listed above, but can also be other values between these content percentages, such as 72.83%; the burnt-out components include carbonaceous components and organic matter. It can be understood that the burnt-out components in some coal gangue also include moisture.
[0037] like Figure 1 , Figure 2 As shown, the method for recycling coal gangue includes the following steps:
[0038] S10: Grind the coal gangue and perform activation treatment at 200°C to 800°C to obtain an activated sample, wherein the burn-out components are burned out during the activation treatment and the carbonaceous components provide heat for the activation process; the obtained activated sample includes silicon and aluminum, and silicon and aluminum exist in the form of amorphous metakaolinite.
[0039] In step S10, the gangue may be ground into powder with a smaller particle size, and then activated, wherein the activation temperature is 200°C to 800°C, such as 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, etc. The main mineral component of the gangue is kaolinite, which will be transformed into amorphous metakaolinite during the activation process, thereby improving the activity of these mineral components in the subsequent acid leaching reaction. Specifically, the chemical reaction equation occurring in this step is as follows:
[0040] Al2O3·2SiO2·2H2O=Al2O3·2SiO2(amorphous)+2H2O↑.
[0041] S20: subjecting the activated sample to an acid leaching reaction with a sulfuric acid solution having a concentration of 1 mol / L to 9 mol / L at a liquid-to-solid ratio of 4 to 10, filtering to obtain a first filtrate and silicon powder, and aluminum element entering the first filtrate; wherein the temperature of the reaction system is 40°C to 100°C.
[0042] In step S20, only one acid leaching reaction is performed. In this step, the liquid-solid ratio of the sulfuric acid solution to the activated sample is 4 to 10, such as 4, 5, 6, 7, 8, 9 or 10, wherein the concentration of the sulfuric acid solution is 1 mol / L to 9 mol / L, such as 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L or 9 mol / L, etc., and the temperature of the reaction system can be controlled at 40°C to 100°C, such as 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C. Specifically, the activated sample can be mixed with sulfuric acid solution at a liquid-solid ratio of 4 to 10, and then stirred to allow the aluminum element to fully react and generate Al2(SO4)3. In this process, since the activated sample has been fully activated, only one acid leaching is required to leach more than 99% of Al2O3, that is, more than 99% of Al2O3 enters the first filtrate, while the silicon element does not participate in the reaction. After solid-liquid separation, it is separated as a precipitate in the filtration, that is, precipitated as silicon micropowder. After simple rinsing and drying, the silicon micropowder is a qualified product that can be used in various fields such as industry. The chemical reaction equation occurring in this step is as follows:
[0043] Al2O3·2SiO2(amorphous)+3H2SO4+aq=Al2(SO4)3+2SiO2↓+3H2O+aq.
[0044] S30: mixing the first filtrate with ammonium sulfate in a molar ratio of ammonia to aluminum of 1:1, performing crystallization after the reaction, and filtering to obtain a second filtrate and ammonium aluminum sulfate.
[0045] In step S30, aluminum element is extracted by ammonium aluminum sulfate. In the molecular formula of ammonium aluminum sulfate NH4Al(SO4)2, the molar ratio of NH4 to Al is 1:1. Therefore, in the present invention, the first filtrate is mixed with ammonium sulfate according to this ratio. Specifically, ammonium sulfate can be added to the first filtrate according to this molar ratio, and stirred to fully dissolve the ammonium aluminum sulfate so that the aluminum element in the first solution can participate in the reaction as much as possible. After the reaction is fully completed, crystallization treatment is performed, and ammonium aluminum sulfate is crystallized. The second filtrate and ammonium aluminum sulfate are obtained by solid-liquid separation. The chemical reaction equation occurring in this process is as follows:
[0046] Al2(SO4)3+(NH4)2SO4+12H2O=2NH4Al(SO4)2·12H2O.
[0047] S40: After the second filtrate is adjusted to the sulfuric acid concentration in step S20, return to step S20.
[0048] In step S40, after the concentration of the second filtrate is adjusted, it can be returned to step S20 as the sulfuric acid solution in step S20, that is, the filtrate after extracting aluminum sulfate ammonia in step S30 can be recycled. In this way, no waste will be generated and no waste of resources will be caused during the entire coal gangue treatment process.
[0049] The method for resource-based treatment of coal gangue provided by the present invention has the following advantages: first, no waste is generated or discharged during the entire process, the comprehensive utilization rate of the main elements aluminum and silicon in the coal gangue is high, and the obtained elements or mixtures can be used as raw materials in industrial production, which can produce good economic benefits, truly realize comprehensive and highly resource-based treatment of coal gangue, and greatly improve the overall utilization value of coal gangue; and there is no secondary waste discharge in the entire process, which is environmentally friendly and realizes the harmless treatment of coal gangue.
[0050] Secondly, by first activating the gangue, the reactivity of its mineral components can be changed. The high-content silicon-aluminum components will be transformed into amorphous kaolinite during the activation process, so that the subsequent acid leaching reaction only needs to be carried out once to achieve an aluminum leaching rate of more than 95%, or even more than 99%; and the requirements for sulfuric acid concentration and reaction system temperature in the acid leaching reaction can be reduced, thereby making the process simpler. At the same time, through the activation treatment, even the organic matter of the burnt-out components in the gangue can be burned off, thereby avoiding its entry into the subsequent acid leaching reaction and causing adverse effects on the reaction, and it can also make full use of the carbonaceous components in the burnt-out to provide a certain amount of heat energy in the activation treatment, thereby saving the requirements for heat energy in the reaction.
[0051] Thirdly, high-purity silicon micropowder can be obtained by filtering after the acid leaching reaction, and the first filtrate obtained by acid leaching can obtain high-purity ammonium aluminum sulfate after reacting with ammonium sulfate and crystallizing, which can be directly used in the food field, water treatment field, etc., and the second filtrate after extracting ammonium aluminum sulfate can also be recycled. It can be seen that the resource treatment method of coal gangue of the present invention can realize the full resource utilization of aluminum and silicon in coal gangue; and only one acid leaching process is required in the process of aluminum extraction, which greatly simplifies the entire aluminum extraction process steps, and can save resources without causing secondary pollution.
[0052] In the coal gangue samples, the main elements aluminum and silicon exist as Al2O3 and SiO2 respectively, and the total amount of the two is more than 70%, among which the content of SiO2 is the highest, followed by the content of Al2O3, and the content of lost components is lower than that of Al2O3. Specifically, SiO2 can reach more than 35%, such as 35%, 36%, 375%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 50% or 52%, etc., and can also be higher; the content of Al2O3 can reach more than 25%, such as 25%, 26%, 28%, 30%, 32%, 35%, 37% or 40%, and can also be higher. The burnt-loss components (including carbonaceous components, organic matter and moisture) in the gangue sample can reach more than 15%, such as 15%, 16%, 18%, 20%, 22%, 23%, 24%, 25%, 26%, 27%, 28% or 30%, etc. Of course, the contents of Al2O3, SiO2 and burnt-loss components are not limited to the percentages listed above, but can also be certain values between these percentages, such as Al2O3 content of 28.52%, SiO2 content of 44.31, and burnt-loss component content of 24.29%, among which the carbonaceous components in the burnt-loss components can provide certain heat energy for the activation process. Coal gangue also includes some other components, such as iron, titanium, calcium, magnesium, potassium, sodium, manganese, phosphorus, etc. Specifically, these elements can exist in the form of oxides such as Fe2O3, TiO2, CaO, MgO, K2O, Na2O, MnO, P2O5, etc. The content of these other components is very low, even negligible. For example, in a coal gangue sample, the content of these elements is 0.39%, 0.60%, 0.67%, 0.11%, 0.07%, 0, 0.05%, and 0.02%, respectively. Most of them enter the first filtrate in step S20, and then enter the second filtrate in step S30.
[0053] In one embodiment, in step S10, the gangue is ground to a particle size less than or equal to 74 μm, such as 74 μm, 72 μm, 70 μm, 65 μm or 60 μm. By first grinding the gangue to a particle size less than or equal to 74 μm, the gangue powder can be activated more fully than the gangue powder ground to other particle size ranges, and the subsequent acid leaching reaction can be more thorough, and the requirements for sulfuric acid concentration, reaction system and other conditions in the subsequent acid leaching reaction can be further reduced. In step S10, the activation treatment time is 30min to 60min, that is, after the coal gangue is ground to a particle size less than or equal to 74μm, the activation treatment is carried out for 30min to 60min, such as 30min, 35min, 40min, 45min, 50min, 55min or 60min, etc. Through the activation treatment for 30min to 60min, the mineral components in the coal gangue can be fully activated, especially the aluminum and silicon components, and the organic matter in the coal gangue can be completely burned away and will not enter the subsequent steps, thereby further increasing the purity of the extracted silicon micropowder and ammonium aluminum sulfate, and the selection of the activation treatment time will not cause waste of energy.
[0054] In a preferred embodiment, in step S20, the concentration of the sulfuric acid solution is 1 mol to 5 mol / L, such as 1 mol, 1.5 mol, 2 mol, 2.5, 3 mol, 3.5 mol, 4 mol, 4.5 mol or 5 mol, etc. Using a sulfuric acid solution in this concentration range can further reduce the use of sulfuric acid and save resources.
[0055] In step S20, the sulfuric acid solution is mixed with the activated sample, such as the activated sample can be added to the sulfuric acid solution, and then stirred, wherein the sulfuric acid solution and the activated sample are stirred and dissolved for 10min to 80min and then filtered, such as the stirring and dissolving time is 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min, 60min, 70min or 80min, etc., by stirring and dissolving for this length of time, the other components in the activated sample except SiO2 can be fully dissolved, especially the aluminum element, after solid-liquid filtration and separation, the leaching rate of aluminum in the first solution is higher, basically all leached, and the purity of the obtained solid silicon micropowder is extremely high, and it can be directly used as an industrial product after simple cleaning.
[0056] Among them, in step S20, the total amount of sulfuric acid is controlled according to the sulfuric acid concentration used and the liquid-solid ratio adopted, wherein the sulfuric acid concentration is negatively correlated with the liquid-solid ratio, that is, the sulfuric acid concentration and the liquid-solid ratio coordinately control the total amount of acid used, and the total amount of acid used can be controlled within a certain range by increasing the sulfuric acid concentration and reducing the liquid-solid ratio, or by reducing the sulfuric acid concentration and increasing the liquid-solid ratio. Specifically, the total amount of acid used can be selected as 1 to 1.6 times the mass of the activated sample, such as the total amount of acid used is equal to the mass of the activated sample, or it can be 1.1 times, 1.2 times, 1.3 times, 1.4 times, 1.5 times or 1.6 times the mass of the activated sample. In this embodiment, by coordinating the control of the sulfuric acid concentration and the liquid-solid ratio, the selection range of sulfuric acid can be increased, and the scope of application of the resource recovery treatment method can be further improved.
[0057] Preferably, in step S20, when the concentration of the sulfuric acid solution is 1 mol to 2 mol / L, the liquid-solid ratio is selected to be 6 to 10; when the concentration of the sulfuric acid solution is 4 mol to 5 mol / L, the liquid-solid ratio is 4 to 5. Specifically, when the concentration of the sulfuric acid solution is any one of 1 mol, 1.2 mol / L, 1.5 mol / L, 1.7 mol / L, 1.8 mol / L or 2 mol / L, the liquid-solid ratio may be preferably one of 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5 or 10; when the concentration of the sulfuric acid solution is any one of 4 mol, 4.2 mol, 4.5 mol, 4.6 mol, 4.8 mol or 5 mol / L, the liquid-solid ratio may be preferably one of 4, 4.3, 4.5, 4.8 or 5. By selecting the above-mentioned sulfuric acid solution concentration and liquid-solid ratio, the reaction rate of the acid leaching reaction can be increased, and the acid leaching rate of the aluminum element can be made higher.
[0058] In step S20, the concentration of sulfuric acid and the temperature of the reaction system will affect the reaction rate, and then affect the time of stirring and dissolving. The higher the concentration and the higher the temperature of the reaction system, the faster the reaction rate and the shorter the time required for stirring and dissolving. For example, when the concentration is fixed, the higher the temperature, the faster the reaction rate and the shorter the stirring and dissolving time; when the concentration is fixed. In a preferred embodiment, in step S20, the concentration of sulfuric acid is 2 mol / L, the liquid-solid ratio of sulfuric acid solution to activated sample is 6, and the temperature of the reaction system is 95°C. The use of this concentration, liquid-solid ratio and reaction system temperature can further improve the reaction rate of the acid leaching reaction, shorten the time of stirring and dissolving, and is conducive to improving the efficiency of coal gangue resource utilization in industrial applications.
[0059] In step S20, the container containing the sulfuric acid solution and the activated sample can be directly heated to keep the temperature of the reaction system at 40°C to 100°C, or the container can be directly placed in a water bath and heated in a water bath to keep the temperature of the reaction system at 40°C to 100°C.
[0060] In step S30, the first filtrate can be tested first to determine the amount of aluminum ions it contains, and then ammonium sulfate is added according to a ratio of 1:1 in the molar ratio of ammonia to aluminum. The first filtrate and ammonium sulfate can be carried out at room temperature. In a preferred embodiment, the reaction system temperature is 40°C-100°C for full reaction to increase the reaction rate of ammonium sulfate and Al2(SO4)3, such as the temperature of the reaction system is 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C. Among them, ammonium sulfate can be added to the first filtrate. In this process, the higher the temperature of the reaction system, the faster the dissolution of ammonium sulfate. Specifically, the temperature of the reaction system can be achieved by directly heating the container containing the first filtrate and ammonium sulfate, or by directly placing the container in a water bath and heating it in a water bath. After the ammonium sulfate is completely dissolved, it is cooled and crystallized, and ammonium aluminum sulfate crystals can be obtained by solid-liquid separation.
[0061] It should be noted that the temperatures of the reaction systems in step S20 and step S30 may be the same or different.
[0062] In one embodiment, in step S30, the first filtrate is placed in a water bath at 40°C to 100°C, ammonium sulfate is added to the first filtrate, stirred to dissolve the ammonium sulfate, and then cooled to crystallize. The stirring time is 10 min to 60 min, such as 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min, so that the ammonium sulfate dissolves and reacts as soon as possible. After the dissolution reaction is completely completed, the mixed solution of ammonium aluminum sulfate and the first filtrate is taken out from the water bath and cooled. As the mixed solution is cooled, the ammonium aluminum sulfate generated in the reaction forms crystals, and then the ammonium aluminum sulfate crystals and the second filtrate are separated by solid-liquid separation. In this way, the entire operation process can be facilitated, especially in step S20, when the temperature of the reaction system is also heated by a water bath, the same water bath and the same container for holding the solution can be used. After completing step S20, step S30 can be directly performed in the same container, and the temperature of the mixed solution is heated evenly at various locations in each step. Even if the reaction system temperatures of step S20 and step S30 are different, they can be conveniently adjusted by controlling the water bath.
[0063] In step S30, after the first filtrate is mixed with ammonium sulfate, crystallization can be carried out by cooling, such as natural cooling, or cooling can be accelerated by a cold water bath. Specifically, the precipitation time of ammonium aluminum sulfate crystallization is related to the temperature of the solution and the concentration of ammonium aluminum sulfate. The lower the temperature, the greater the concentration of ammonium aluminum sulfate, the more conducive to the crystallization of ammonium aluminum sulfate, and the shorter the precipitation time. The concentration in this step is specifically determined by the aforementioned acid leaching step. When the leaching rate of aluminum does not change much, the smaller the liquid-to-solid ratio in the above step S20, the aluminum concentration in the acid leaching solution will respond to increase. When the concentration of the acid leaching solution is constant, the crystallization in step S30 is mainly affected by temperature. The lower the temperature, the lower the solubility of ammonium aluminum sulfate, and the more conducive to the precipitation of ammonium aluminum sulfate. In one embodiment, after ammonium sulfate and the first filtrate are mixed and reacted, the reacted solution is allowed to stand at room temperature for 0.5h to 3h, and ammonium aluminum sulfate crystals are obtained after filtration. If the temperature of the reaction system is 40°C to 100°C, ammonium aluminum sulfate will be generated in the solution after ammonium sulfate is fully dissolved in the first filtrate. Thereafter, the solution can be allowed to stand at room temperature for 0.5h, 0.6h, 0.8h, 1h, 1.2h, 1.5h, 1.8h, 2h, 2.2h, 2.5h, 2.8h or 3h. Cooling at room temperature is simple to operate, and the precipitation time of ammonium aluminum sulfate will not be too long, which is beneficial to the industrial implementation of the entire coal gangue resource processing method.
[0064] Among them, when the second filtrate in step S40 is circulated for the first few times, the ammonium aluminum sulfate crystals in step S30 can obtain high-purity ammonium aluminum sulfate by only sequential crystallization treatment, which can be directly used as a finished product in industries and other fields. As the number of cycles of step S40 increases, in order to obtain higher-purity ammonium aluminum sulfate crystals, the ammonium aluminum sulfate obtained in step S30 can be crystallized multiple times. In one embodiment, after step S40 is circulated for a preset number of times, the ammonium aluminum sulfate crystals obtained in step S30 are recrystallized 1 to 2 times to obtain the finished ammonium aluminum sulfate. In this way, the use of new sulfuric acid solution in step S20 can be reduced, and the purity of the extracted ammonium aluminum sulfate crystals can be guaranteed.
[0065] The present invention also provides a coal gangue resource utilization system, which is used to implement any of the coal gangue resource processing methods described above. Specifically, the coal gangue resource utilization system includes:
[0066] A grinding device for grinding in step S10, an activation device for activation treatment in step S10, a mixing reaction device for acid leaching reaction in step S20 and reaction in step S30, and a filtering and separation device for filtering in steps S20 and S30.
[0067] The resource recovery method of the present invention is described below with reference to specific embodiments.
[0068] Example 1
[0069] The coal gangue of this embodiment has a SiO2 content of 44.31% and an Al2O3 content of 28.52%. The method for recycling coal gangue includes the following steps:
[0070] S10: Grinding the coal gangue powder to a particle size of 74 μm, and then activating the powder at 600° C. for 40 min to obtain an activated sample;
[0071] S20: placing the activated sample obtained in S10 in a sulfuric acid solution with a concentration of 1.5 mol / L and a temperature of 70° C. at a liquid-to-solid ratio of 10, stirring and dissolving for 60 min, and filtering to obtain silicon micropowder and a first filtrate;
[0072] S30: placing the first filtrate in a water bath at 90° C., then adding ammonium sulfate to the first filtrate, performing crystallization treatment after the reaction, and filtering and separating to obtain a second filtrate and ammonium aluminum sulfate;
[0073] S40: After the second filtrate is adjusted to a sulfuric acid concentration of 1.5 mol / L, the process returns to step S20.
[0074] After analysis and testing, the silicon micropowder and ammonium aluminum sulfate obtained in the above steps can meet the relevant industry standards, and the leaching rate of aluminum in the first filtrate reaches 98.52%.
[0075] Example 2
[0076] The coal gangue of this embodiment has the same composition as that of embodiment 1, and the method for recycling coal gangue comprises the following steps:
[0077] S10: Grinding the coal gangue powder to a particle size of 74 μm, and then activating the powder at 800° C. for 40 min to obtain an activated sample;
[0078] S20: placing the activated sample obtained in S10 in a sulfuric acid solution with a concentration of 9 mol / L and a temperature of 40° C. at a liquid-to-solid ratio of 4, stirring and dissolving for 30 min, and filtering to obtain silicon micropowder and a first filtrate;
[0079] S30: placing the first filtrate in a water bath at 80° C., then adding ammonium sulfate to the first filtrate, performing crystallization treatment after the reaction, and filtering and separating to obtain a second filtrate and ammonium aluminum sulfate;
[0080] S40: After the second filtrate is adjusted to a sulfuric acid concentration of 9 mol / L, the process returns to step S20.
[0081] After analysis and testing, the silicon micropowder and ammonium aluminum sulfate obtained in the above steps can meet the relevant industry standards, and the leaching rate of aluminum in the first filtrate reaches 97.21%.
[0082] Example 3
[0083] In the coal gangue of this embodiment, the SiO2 content is 42.26%, and the Al2O3 content is 30.15%. The coal gangue resource processing method comprises the following steps:
[0084] S10: Grinding the coal gangue powder to a particle size of 74 μm, and then activating the powder at 400° C. for 60 min to obtain an activated sample;
[0085] S20: placing the activated sample obtained in S10 in a sulfuric acid solution with a concentration of 2 mol / L and a temperature of 50° C. at a liquid-to-solid ratio of 8, stirring and dissolving for 50 min, and filtering to obtain silicon micropowder and a first filtrate;
[0086] S30: placing the first filtrate in a water bath at 85° C., then adding ammonium sulfate to the first filtrate, performing crystallization treatment after the reaction, and filtering and separating to obtain a second filtrate and ammonium aluminum sulfate;
[0087] S40: After the second filtrate is adjusted to a sulfuric acid concentration of 2 mol / L, the process returns to step S20.
[0088] After analysis and testing, the silicon micropowder and ammonium aluminum sulfate obtained in the above steps can meet the relevant industry standards, and the leaching rate of aluminum in the first filtrate reaches 95.42%.
[0089] Example 4
[0090] The gangue of this embodiment has the same composition as the gangue in Embodiment 2. The gangue resource processing method includes the following steps:
[0091] S10: Grinding the coal gangue powder to a particle size of 74 μm, and then activating the powder at 200° C. for 60 min to obtain an activated sample;
[0092] S20: placing the activated sample obtained in S10 in a sulfuric acid solution with a concentration of 5 mol / L and a temperature of 100° C. at a liquid-to-solid ratio of 6, stirring and dissolving for 50 min, and filtering to obtain silicon micropowder and a first filtrate;
[0093] S30: placing the first filtrate in a water bath at 60° C., then adding ammonium sulfate to the first filtrate, performing crystallization treatment after the reaction, and filtering and separating to obtain a second filtrate and ammonium aluminum sulfate;
[0094] S40: After the second filtrate is adjusted to a sulfuric acid concentration of 5 mol / L, the process returns to step S20.
[0095] After analysis and testing, the silicon micropowder and ammonium aluminum sulfate obtained in the above steps can meet the relevant industry standards, and the leaching rate of aluminum in the first filtrate reaches 96.83%.
[0096] Example 5
[0097] The gangue of this embodiment has the same composition as the gangue in Embodiment 2. The gangue resource processing method includes the following steps:
[0098] S10: Grinding the coal gangue powder to a particle size of 74 μm, and then activating the powder at 700° C. for 50 min to obtain an activated sample;
[0099] S20: placing the activated sample obtained in S10 in a sulfuric acid solution with a concentration of 6 mol / L and a temperature of 95° C. at a liquid-to-solid ratio of 6, stirring and dissolving for 50 min, and filtering to obtain silicon micropowder and a first filtrate;
[0100] S30: placing the first filtrate in a water bath at 95° C., then adding ammonium sulfate to the first filtrate, performing crystallization treatment after the reaction, and filtering and separating to obtain a second filtrate and ammonium aluminum sulfate;
[0101] S40: After the second filtrate is adjusted to a sulfuric acid concentration of 6 mol / L, the process returns to step S20.
[0102] After analysis and testing, the silicon micropowder and ammonium aluminum sulfate obtained in the above steps can meet the relevant industry standards, and the leaching rate of aluminum in the first filtrate reaches 99.07%.
[0103] Those skilled in the art will appreciate that, without conflict, the above-mentioned preferred solutions can be freely combined and superimposed.
[0104] It should be understood that the above-mentioned embodiments are merely illustrative and not restrictive. Without departing from the basic principles of the present invention, various obvious or equivalent modifications or substitutions that can be made by those skilled in the art to the above-mentioned details will all be included in the scope of the claims of the present invention.
Claims
1. A method for recycling coal gangue, wherein the coal gangue comprises silicon, aluminum and a burnt-out component, the sum of the oxide contents of silicon and aluminum is greater than or equal to 70%, and the burnt-out component comprises a carbonaceous component and an organic matter; characterized in that: Includes steps: S10: grinding the gangue, and performing activation treatment at 200° C. to 800° C. to obtain an activated sample, wherein the burn-out component is burned out during the activation treatment, and the carbonaceous component provides heat for the activation process; the obtained activated sample includes silicon and aluminum, and the silicon and aluminum mainly exist in the form of amorphous metakaolinite; S20: subjecting the activated sample to an acid leaching reaction with a sulfuric acid solution having a concentration of 1 to 9 mol / L at a liquid-to-solid ratio of 4 to 10, filtering to obtain a first filtrate and silicon powder, wherein the aluminum element enters the first filtrate; wherein the temperature of the reaction system is 40° C. to 100° C.; S30: mixing the first filtrate with ammonium sulfate in a ratio of ammonia to aluminum of 1:1, performing crystallization after the reaction, and filtering to obtain a second filtrate and ammonium aluminum sulfate; S40: After adjusting the second filtrate to the sulfuric acid concentration in step S20, return to step S20.
2. The method for recycling coal gangue according to claim 1, characterized in that: In the step S10, the coal gangue is ground to a particle size less than or equal to 74 μm; and the activation treatment time is 30 min to 60 min.
3. The method for recycling coal gangue according to claim 1, characterized in that: In the step S20, the concentration of the sulfuric acid solution is 1 mol to 5 mol / L, and the sulfuric acid solution and the activated sample are stirred and dissolved for 10 min to 80 min and then filtered.
4. The method for recycling coal gangue according to claim 1, characterized in that: In the step S20, the total amount of sulfuric acid is controlled according to the sulfuric acid concentration and the liquid-to-solid ratio, wherein the sulfuric acid concentration is negatively correlated with the liquid-to-solid ratio.
5. The method for recycling coal gangue according to claim 1, characterized in that: In the step S20, When the concentration of the sulfuric acid solution is 1 mol to 2 mol / L, the liquid-to-solid ratio is 6 to 10; When the concentration of the sulfuric acid solution is 4 mol to 5 mol / L, the liquid-to-solid ratio is 4 to 5.
6. The method for recycling coal gangue according to claim 1, characterized in that: In the step S20, the concentration of the sulfuric acid is 2 mol / L; the liquid-to-solid ratio of the sulfuric acid solution to the activated sample is 6; and the temperature of the reaction system is 95°C.
7. The method for recycling coal gangue according to claim 1, characterized in that: In the step S30, the first filtrate is placed in a water bath at 40°C to 100°C, ammonium sulfate is added thereto, stirred to dissolve the ammonium sulfate, and then cooled to crystallize.
8. The method for recycling coal gangue according to claim 1, characterized in that: In the step S30, the solution after the reaction is allowed to stand at room temperature for 0.5 h to 3 h, and then filtered to obtain ammonium aluminum sulfate crystals.
9. The method for recycling coal gangue according to any one of claims 1 to 8, characterized in that: After the step S40 is cycled for a preset number of times, the ammonium aluminum sulfate crystals obtained in the step S30 are recrystallized 1 to 2 times to obtain a finished ammonium aluminum sulfate product.
10. A coal gangue resource utilization system, used for implementing the coal gangue resource processing method according to any one of claims 1 to 9; characterized in that: include: A grinding device for grinding in step S10, an activation device for activation treatment in step S10, a mixing reaction device for acid leaching reaction in step S20 and reaction in step S30, and a filtering and separation device for filtering in steps S20 and S30.