High-purity low-chlorine low-aluminum-calcium nano lutetium oxide powder and preparation method thereof
By adjusting the concentration and pH value of the lutetium feed liquid and precipitant, combined with multiple precipitations and high-temperature treatments, the problem of impurity content and particle size distribution in rare earth lutetium oxide powder was solved, and high-purity, low-impurity, nanometer-sized lutetium oxide was prepared. Powders to meet the needs of high-performance applications.
Patent Information
- Application Number
- CN202410744579.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology is difficult to effectively control the impurity content in rare earth lutetium oxide powder, especially Al, Ca, and Cl, and the nanometer size and particle size distribution are uneven, making it unable to meet the application requirements of high purity and high performance.
By adjusting the Lu3+ ion concentration and pH value in the lutetium feed solution, using citric acid and oxalic acid as precipitants, performing two precipitations and high-temperature burning, combined with stirring rate control, a high-purity, low-chlorine, low-aluminum calcium nano-oxide was prepared Lutetium powder ensures that CaO<5ppm, Al2O3<15ppm, Cl-<10ppm, the powder size is 250~300nm, and the crystal phase structure is cubic phase.
It achieves high purity, low impurity content and uniform particle size distribution of nano-lutetium oxide, provides a simple and low-cost preparation process, meets the needs of high-performance applications, and improves the economic value of the finished product.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of rare earth materials and relates to a high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder and a preparation method thereof. Background Art
[0002] Due to its unique physical and chemical properties, rare earth lutetium oxide powder is widely used in many fields, including as an additive element of yttrium iron and yttrium aluminum garnet, active material of phosphor, and additive for making special alloys, magnetic materials and phosphor. There are various methods for preparing lutetium oxide powder, including liquid phase method, solid phase method, ultrasonic crushing method, low temperature crushing method, explosion method, mechanical alloying method (high energy ball milling method) and solid phase thermal decomposition method. Among them, the most commonly used precipitation method is to add the precipitant and the salt solution of rare earth by different feeding methods and control the process conditions to obtain the precursor, and then wash, dry and calcine to obtain rare earth oxide. This method is a low-cost and high-efficiency method for preparing rare earth oxide powder.
[0003] Patent CN115536053A discloses a method for preparing low-chloride high-purity lutetium oxide, comprising the following steps: in a P507-kerosene-HCl or naphthenic acid-kerosene-HCl extraction system, a rare earth extractant fully loaded with lutetium enters a continuous extraction tank, nitric acid is used as a stripping agent, lutetium nitrate is obtained in the raffinate liquid, and then oxalic acid precipitant is added for precipitation reaction to obtain lutetium oxalate precipitate, which is then calcined at high temperature to obtain the low-chloride lutetium oxide. The chloride ion content is ≤10ppm.
[0004] Patent CN110372027A discloses a method for precipitating low-chloride lutetium oxide in a chloride system, comprising the following steps: (1) preparing a feed solution: mixing a LuCl3 solution with a concentration of 0.1 to 0.8 mol / L with a concentrated nitric acid solution to form a feed solution with a stable concentration, wherein the nitrate concentration in the feed solution is 0.3 to 2.0 mol / L; (2) preparing a precipitant: using an oxalic acid solution with a concentration of 120 to 150 g / L, heating the solution until solid oxalic acid is present in the oxalic acid solution. The acid is completely dissolved, thereby preparing the required precipitant; (3) precipitation to remove chloride ions: adopting a parallel flow precipitation method, the bottom water, the above-mentioned feed liquid and the above-mentioned precipitant are mixed and reacted at a temperature of 35-60°C for precipitation, so that the stoichiometric ratio of lutetium chloride and oxalic acid put into the reaction is n (lutetium chloride): n (oxalic acid) = 1: (1.65-1.95); (4) washing to remove chloride ions: washing the precipitated lutetium oxalate; (5) calcination: calcining the washed precipitated lutetium oxalate to obtain a low-chloride lutetium oxide product. This can effectively prevent the problem of chloride ion encapsulation and the problem of high impurities caused by powder agglomeration during the precipitation of lutetium oxalate.
[0005] Patent CN111874937A discloses a method for preparing low-chlorine lutetium oxide, which reduces the content of chloride ions in lutetium oxide and prepares high-purity, low-chlorine lutetium oxide; the method comprises the following steps: (1) reacting a lutetium chloride feed liquid with an oxalic acid solution, the reaction temperature being controlled at 60°C, aging the solution at 60°C for 2h after the feed is completed, and then filtering to obtain a precipitate A; (2) calcining the precipitate A at high temperature, cooling it, adding concentrated nitric acid to dissolve it, and then diluting it with high-purity water A 0.5 mol / L lutetium nitrate solution is obtained; (3) the lutetium nitrate solution is reacted with the oxalic acid solution, the reaction temperature is controlled at 60°C, and then after standing to clarify, it is aged at 60°C for 30 minutes and then filtered while hot to obtain a precipitate, and then the precipitate is washed 1 to 2 times with 60°C high-purity water to obtain a lutetium oxalate precipitate; (4) the lutetium oxalate precipitate is dried, microwave-heated to 800°C, kept warm for 1 to 2 hours, and naturally cooled to room temperature to obtain low-chlorine lutetium oxide. The two-step precipitation method is used for precipitation, and the chloride ion content of the burned lutetium oxide is less than 20ppm, and other impurities such as chlorine are also relatively reduced, and the purity reaches more than 99.999%.
[0006] The article "Preparation of small-particle lutetium oxide powder, Zhong Kexiang et al., Fujian Metallurgy" dissolves high-purity lutetium oxide powder in hydrochloric acid according to the required weight to prepare lutetium chloride solution, uses ammonium oxalate solution as a precipitant, and uses a reverse precipitation method to obtain a lutetium oxalate precursor, which is then calcined to obtain lutetium oxide powder. Under optimal conditions, this method can be used to prepare lutetium oxide powder with a D50 between 1.0 and 2.0 μm.
[0007] Common impurities in rare earth oxide powders are usually Al, Ca, and Cl. Due to their particularity, it is much more difficult to reduce their content than rare earth impurities (Pr, Nd, Sm, etc.) and metal element impurities (Cu, Fe, Si, etc.). In addition, different applications have different requirements for the particle size of lutetium oxide powder, and precise control of particle size is a challenge in the preparation process. With the trend of high-quality development in my country, the requirements for the purity and impurity content of rare earth oxides are becoming more and more stringent. Not only the purity and impurities need to be controlled, but also the size and morphology of lutetium oxide fragments need to be strictly controlled; the demand for nano-sized lutetium oxide is also increasing. Summary of the invention
[0008] Based on the needs and deficiencies of the prior art, the present invention provides a high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder and a preparation method thereof. The prepared lutetium oxide product contains CaO < 5ppm, Al2O3 < 15ppm, Cl - <10ppm, powder size is 250-300nm, and the crystal structure is cubic. Through the adjustment of the process and the control of the parameters, lutetium oxide with nano-particle size, narrow particle size distribution, low impurity content and good crystallinity is prepared.
[0009] In order to achieve the purpose of the present invention, the present invention provides the following technical solutions: A method for preparing high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder comprises the following steps: (1) Control and adjust Lu in lutetium solution 3+ Ion concentration According to the Lu in the lutetium solution 3+ The concentration is diluted with deionized water or heated to evaporate the water, and the concentration of lutetium chloride is controlled to be 40-45 g / L, and then the pH is adjusted to 4.6-4.8 with sodium hydroxide; 70-75 g of citric acid and 10-15 g of cyclohexanediaminetetraacetic acid are weighed, dissolved and diluted to 1 L with deionized water, and a citric acid aqueous solution with a concentration of 70-75 g / L is prepared; 60-65 g of industrial refined oxalic acid and 1-2 g of cocamidopropyl betaine are weighed, dissolved and diluted to 1 L with deionized water, and a refined oxalic acid aqueous solution with a concentration of 60-65 g / L is prepared; (2) First positive precipitation Pour the lutetium solution into the reactor, heat it to 45-50°C and keep it there, while turning on the stirrer; Add citric acid aqueous solution to the reactor, and add 1L of citric acid aqueous solution in 20 to 25 minutes until the precipitation reaction is complete; continue stirring for 3 to 5 minutes, then stop stirring and let stand for phase separation; (3) Precipitation and dissolution Dissolve the solid phase in step (2) with hydrochloric acid, then add deionized water to dilute it. 3+ Ion concentration is 35-40 g / L; (4) Second anti-precipitation Pour the purified oxalic acid aqueous solution in step (1) into the reactor, heat it to 50-55°C and maintain it, while turning on the stirrer; add the lutetium solution in step (3) into the reactor, and add 1L of the lutetium solution in 30-35 minutes until the precipitation reaction is complete; continue stirring for 3-5 minutes, then stop stirring and let stand for phase separation; (5) Preparation of Lutetium Oxide Finished Product Extract the mother liquor of oxalic acid precipitation in step (4), place the precipitate in a suction filtration device and filter and rinse it with hot water at 50-55°C for 3-5 times, each time for 15-20 minutes; then dehydrate and filter, put the washed lutetium oxalate into a crucible, and burn it in a high-temperature furnace at 850-950°C for more than 2 hours; thus, a lutetium oxide product is obtained; (6) Grinding and screening The lutetium oxide product obtained in step (5) is ground and sieved to obtain high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder.
[0010] Furthermore, the stirring rate in step (2) is 70 to 90 r / min. -1 .
[0011] Furthermore, the stirring rate in step (4) is 40 to 50 r / min. -1 .
[0012] Since the precipitate needs to be dissolved in an acid solution after the positive precipitation in step (2), the dispersion and morphology of the precipitate at this time have little effect on the subsequent finished product. In order to improve the reaction efficiency, the stirring rate can be set faster to improve the precipitation reaction efficiency. Preferably, the stirring rate in step (2) is 80 to 90 r / min -1 .
[0013] Since the reverse precipitation in step (4) is an important factor in determining the size and morphology of the finished product, the stirring rate is set to a lower level for control. Preferably, the stirring rate in step (4) is 40 to 45 r / min. -1 .
[0014] The cyclohexanediaminetetraacetic acid added to the precipitant citric acid solution in step (2) has a good complexing effect on Ca and Al ions, effectively reducing the impurity ions entering the second reverse precipitation process, thereby reducing the impurity ions entering the burning step.
[0015] The cocamidopropyl betaine surfactant added to the precipitant oxalic acid aqueous solution in step (4) can effectively reduce the surface tension of the lutetium solution when added, improve the dispersibility of the rare earth precipitate, and help control its morphology.
[0016] The main components of the lutetium solution are one or more of lutetium chloride and lutetium nitrate; in addition to lutetium, it also contains trace amounts of rare earth element impurities such as La, Ce~Yb, Y, etc., and the total content thereof is less than 50ppm.
[0017] A high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder is prepared by the above method, and by weight, TREO>99.6%, Lu2O3 / TREO>99.995%, Yb2O3<10ppm, other single rare earth impurities<1.0ppm, SiO2<10ppm, CaO<5ppm, Al2O3<15ppm, Cl - <10ppm, powder size is 250~300nm, and the crystal structure is cubic phase.
[0018] The method for preparing a high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder provided by the present invention has the following beneficial effects compared with the prior art: (1) It provides a simple and low-cost preparation process for the preparation of nano-lutetium oxide with narrow and uniform nano-size distribution.
[0019] (2) The prepared nano-lutetium oxide has high purity and low impurity ion content, which can meet high-performance application scenarios and needs and has good economic value.
[0020] (3) The present invention improves and optimizes the precipitation process for preparing rare earth oxides. Compared with the related schemes of the prior art, the present invention has obvious advantages in some aspects. The raw material can come from a lutetium solution with lower purity. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Example 1
[0022] The lutetium solution is a lutetium chloride solution, the lutetium chloride concentration is 50 g / L, the content of rare earth element impurities such as La, Ce~Yb, Y is less than 20 ppm, CaO is less than 20 ppm, and the Al2O3 content is greater than 40 ppm.
[0023] A method for preparing high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder comprises the following steps: (1) Control and adjust Lu in lutetium solution 3+ Ion concentration According to the Lu in the lutetium solution 3+ The concentration was diluted with deionized water to control the concentration to 40 g / L, and then the pH was adjusted to 4.6 with sodium hydroxide; 70 g of citric acid and 10 g of cyclohexanediaminetetraacetic acid were weighed, dissolved and diluted to 1 L with deionized water to prepare a citric acid aqueous solution with a concentration of 70 g / L; 60 g of industrial refined oxalic acid and 1 g of cocamidopropyl betaine were weighed, dissolved and diluted to 1 L with deionized water to prepare a refined oxalic acid aqueous solution with a concentration of 60 g / L; (2) First positive precipitation Pour the lutetium solution into the reactor, heat it to 45°C and keep it, while turning on the stirrer; add citric acid aqueous solution to the reactor, and add 1L of citric acid aqueous solution in 20 minutes until the precipitation reaction is complete; continue stirring for 3 minutes, then stop stirring and let it stand for phase separation; (3) Precipitation and dissolution Dissolve the solid phase in step (2) with hydrochloric acid, then add deionized water to dilute it. 3+ The ion concentration is 35g / L; (4) Second anti-precipitation Pour the purified oxalic acid aqueous solution in step (1) into the reactor, heat it to 50°C and keep it at this temperature, while turning on the stirrer; add the lutetium solution in step (3) into the reactor, and add 1L of the lutetium solution in 30 minutes until the precipitation reaction is complete; continue stirring for 3 to 5 minutes, then stop stirring and let stand for phase separation; (5) Preparation of Lutetium Oxide Finished Product The mother liquor water of the oxalic acid precipitation in step (4) is extracted, and the precipitate is placed in a suction filtration device and filtered and rinsed with 50°C hot water for 3 times, each time for 15 minutes; then the precipitate is dehydrated and filtered, and the washed lutetium oxalate is placed in a crucible and calcined in a high-temperature furnace at 850°C for 6 hours; thus, the lutetium oxide product is obtained.
[0024] (6) Grinding and screening Grinding and sieving the lutetium oxide product obtained in step (5) to obtain high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder; Wherein, the stirring rate in step (2) is 70 r·min -1 .
[0025] Wherein, the stirring rate in step (4) is 40 r·min -1 . Example 2
[0026] The lutetium solution is a lutetium chloride solution, the lutetium chloride concentration is 30 g / L, the content of rare earth element impurities such as La, Ce~Yb, Y is less than 10 ppm, CaO is less than 30 ppm, and the Al2O3 content is greater than 30 ppm.
[0027] A method for preparing high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder comprises the following steps: (1) Control and adjust Lu in lutetium solution 3+ Ion concentration According to the Lu in the lutetium solution 3+ Heat the solution to evaporate water and control its concentration to 50 g / L, then adjust the pH to 4.8 with sodium hydroxide; weigh 75 g of citric acid and 15 g of cyclohexanediaminetetraacetic acid, dissolve them in deionized water and dilute to 1 L to prepare a citric acid aqueous solution with a concentration of 75 g / L; weigh 65 g of industrial refined oxalic acid and 2 g of cocamidopropyl betaine, dissolve them in deionized water and dilute to 1 L to prepare a refined oxalic acid aqueous solution with a concentration of 65 g / L; (2) First positive precipitation Pour the lutetium solution into the reactor, heat it to 50°C and keep it, while turning on the stirrer; add citric acid aqueous solution to the reactor, and add 1L of citric acid aqueous solution in 25 minutes until the precipitation reaction is complete; continue stirring for 5 minutes, then stop stirring and let it stand for phase separation; (3) Precipitation and dissolution Dissolve the solid phase in step (2) with hydrochloric acid or nitric acid, and then add deionized water to dilute it. 3+ The ion concentration is 40g / L; (4) Second anti-precipitation Pour the purified oxalic acid aqueous solution in step (1) into the reactor, heat it to 55°C and keep it at this temperature, while turning on the stirrer; add the lutetium solution in step (3) into the reactor, and add 1L of the lutetium solution in 35 minutes until the precipitation reaction is complete; continue stirring for 5 minutes, then stop stirring and let stand for phase separation; (5) Preparation of Lutetium Oxide Finished Product Extract the mother liquor of oxalic acid precipitation in step (4), place the precipitate in a suction filtration device and filter and rinse it with 55°C hot water for 5 times, each time for 20 minutes; then dehydrate and filter, put the washed lutetium oxalate into a crucible, and burn it in a high-temperature furnace at 950°C for 8 hours; thus, the lutetium oxide product is obtained; (6) Grinding and screening The lutetium oxide product obtained in step (5) is ground and sieved to obtain high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder.
[0028] Wherein, the stirring rate in step (2) is 90 r·min -1 .
[0029] Wherein, the stirring rate in step (4) is 50 r·min -1 . Example 3
[0030] The lutetium solution is lutetium chloride and lutetium nitrate, which are the waste liquid of our laboratory. 3+ The concentration is 10g / L, the content of rare earth element impurities such as La, Ce~Yb, Y is <30ppm, CaO is <40ppm, and Al2O3 content is >200ppm.
[0031] A method for preparing high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder comprises the following steps: (1) Control and adjust Lu in lutetium solution 3+ Ion concentration According to the Lu in the lutetium solution 3+ Concentrated heating evaporates water to control its concentration to 44 g / L, and then adjusts the pH to 4.7 with sodium hydroxide and hydrochloric acid; weighs 73 g of citric acid and 13 g of cyclohexanediaminetetraacetic acid, dissolves them in deionized water and dilutes them to 1 L to prepare a citric acid aqueous solution with a concentration of 73 g / L; weighs 63 g of industrial refined oxalic acid and 1.8 g of cocamidopropyl betaine, dissolves them in deionized water and dilutes them to 1 L to prepare a refined oxalic acid aqueous solution with a concentration of 63 g / L; (2) First positive precipitation Pour the lutetium solution into the reactor, heat it to 48°C and keep it, while turning on the stirrer; add citric acid aqueous solution to the reactor, and add 1L of citric acid aqueous solution in 24 minutes until the precipitation reaction is complete; continue stirring for 4 minutes, then stop stirring and let it stand for phase separation; (3) Precipitation and dissolution Dissolve the solid phase in step (2) with hydrochloric acid, then add deionized water to dilute it. 3+ The ion concentration is 38g / L; (4) Second anti-precipitation Pour the purified oxalic acid aqueous solution in step (1) into the reactor, heat it to 53°C and keep it at this temperature, while turning on the stirrer; add the lutetium solution in step (3) into the reactor, and add 1L of the lutetium solution in 33 minutes until the precipitation reaction is complete; continue stirring for 4 minutes, then stop stirring and let stand for phase separation; (5) Preparation of Lutetium Oxide Finished Product Extract the mother liquor of oxalic acid precipitation in step (4), place the precipitate in a suction filtration device and filter and rinse it with 54°C hot water for 4 times, each time for 18 minutes; then dehydrate and filter, put the washed lutetium oxalate into a crucible, and burn it in a high-temperature furnace at 900°C for 10 hours; thus, the lutetium oxide product is obtained; (6) Grinding and screening The lutetium oxide product obtained in step (5) is ground and sieved to obtain high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder.
[0032] Furthermore, the stirring rate in step (2) is 80 r / min -1 .
[0033] Furthermore, the stirring rate in step (4) is 45 r / min -1 . Example 4
[0034] The lutetium feed solution is a lutetium nitrate solution, the lutetium nitrate concentration is 70g / L, the content of rare earth element impurities such as La, Ce~Yb, Y is less than 20ppm, CaO is less than 30ppm, and Al2O3 content is greater than 60ppm.
[0035] A method for preparing high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder comprises the following steps: (1) Control and adjust Lu in lutetium solution 3+ Ion concentration According to the Lu in the lutetium solution 3+ The concentration was diluted with deionized water to control the concentration to 43 g / L, and then the pH was adjusted to 4.7 with sodium hydroxide and hydrochloric acid; 72 g of citric acid and 12 g of cyclohexanediaminetetraacetic acid were weighed, dissolved and diluted to 1 L with deionized water to prepare a citric acid aqueous solution with a concentration of 72 g / L; 62 g of industrial refined oxalic acid and 1.2 g of cocamidopropyl betaine were weighed, dissolved and diluted to 1 L with deionized water to prepare a refined oxalic acid aqueous solution with a concentration of 62 g / L; (2) First positive precipitation Pour the lutetium solution into the reactor, heat it to 47°C and keep it, while turning on the stirrer; add citric acid aqueous solution to the reactor, and add 1L of citric acid aqueous solution in 22 minutes until the precipitation reaction is complete; continue stirring for 4 minutes, then stop stirring and let it stand for phase separation; (3) Precipitation and dissolution Dissolve the solid phase in step (2) with hydrochloric acid, then add deionized water to dilute it. 3+ The ion concentration is 36g / L; (4) Second anti-precipitation Pour the purified oxalic acid aqueous solution in step (1) into the reactor, heat it to 52°C and keep it at this temperature, while turning on the stirrer; add the lutetium solution in step (3) into the reactor, and add 1L of the lutetium solution in 32 minutes until the precipitation reaction is complete; continue stirring for 4 minutes, then stop stirring and let stand for phase separation; (5) Preparation of Lutetium Oxide Finished Product Extract the mother liquor of oxalic acid precipitation in step (4), place the precipitate in a suction filtration device and filter and rinse it with hot water at 50-55°C for 4 times, each time for 17 minutes; then dehydrate and filter, put the washed lutetium oxalate into a crucible, and burn it in a high-temperature furnace at 900°C for 10 hours; thus, a lutetium oxide product is obtained; (6) Grinding and screening The lutetium oxide product obtained in step (5) is ground and sieved to obtain high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder.
[0036] Furthermore, the stirring rate in step (2) is 80 r / min -1 .
[0037] Furthermore, the stirring rate in step (4) is 45 r / min -1 .
[0038] In order to investigate the influence of process parameters on the properties of lutetium oxide products, we used Example 4 as a benchmark and adjusted the single factor level as a control group.
[0039] Comparative Example 1 Comparative Example 1 is substantially the same as Example 4, except that cyclohexanediaminetetraacetic acid is not added to the citric acid aqueous solution in Comparative Example 1.
[0040] Comparative Example 2 Comparative Example 2 is substantially the same as Example 4, except that in Comparative Example 2, no cocamidopropyl betaine is added to the refined oxalic acid aqueous solution.
[0041] Comparative Example 3 Comparative Example 3 is basically the same as Example 4, except that step (4) in Comparative Example 3 adopts positive precipitation; that is, the lutetium solution in step (2) is poured into a reactor, heated to 52° C. and maintained, and the agitator is turned on at the same time; the refined oxalic acid aqueous solution in step (1) is added to the reactor, and 1L of lutetium solution is added with the refined oxalic acid aqueous solution in 32 minutes until the precipitation reaction is complete; stirring is continued for 4 minutes, then stirring is stopped and the phases are allowed to stand for separation.
[0042] The morphology of the lutetium oxide powders prepared in Examples 1-4 and Comparative Examples 1-3 was observed by scanning electron microscopy and their grain sizes were measured. The specific data are recorded in Table 1.
[0043] Table 1 Example 1 Example 2 Example 3 Example 4 Grain size (nm) 257 289 268 274 Comparative Example 1 Comparative Example 2 Comparative Example 3 Grain size (nm) 265 846 1240 It can be seen from the experimental data that the lutetium oxide powder crystals prepared in Examples 1-4 have small grains, uniform particle size, good dispersibility, and are nano-scale, indicating that the lutetium oxide prepared by the present invention is nano-lutetium oxide; the lutetium oxide powder grain size of Comparative Example 1 is the same as that of Example 4, indicating that the precipitant used in the first positive precipitation has little effect on the grain size; however, the lutetium oxide powder grain size of Comparative Example 2 is much larger than that of Example 4, which indicates that adding cocamidopropyl betaine to the precipitant can reduce precipitation agglomeration and help improve dispersibility. In addition, since both positive precipitations are used in Comparative Example 3, the lutetium oxide powder grain size obtained is 1240nm, i.e., 1.2μm, which is no longer nano-grade lutetium oxide in a strict sense. It can be seen that the second reverse precipitation step has a decisive influence on the size of the lutetium oxide powder. This is also consistent with the research conclusions of the prior art; when the precipitant is reversed, the pH value in the solution remains basically unchanged, the nucleation rate is greater than the growth rate, and it is conducive to the growth of small particles.
[0044] The lutetium oxide products of Examples 1-4 and Comparative Examples 1-3 were analyzed and tested, and the specific test data are recorded in Tables 2-3.
[0045] Table 2 Inspection items unit Example 1 Example 2 Example 3 Example 4 TREO % 99.71 99.65 99.68 99.73 LOI % 0.28 0.30 0.30 0.32 <![CDATA[Lu2O3 / TREO]]> % 99.997 99.996 99.999 99.998 <![CDATA[La2O3]]> ppm <1 <1 <1 <1 <![CDATA[CeO2]]> ppm <1 <1 <1 <1 <![CDATA[Pr6O 11 ]]> ppm <1 <1 <1 <1 <![CDATA[Nd2O3]]> ppm <1 <1 <1 <1 <![CDATA[Sm2O3]]> ppm <1 <1 <1 <1 <![CDATA[Eu2O3]]> ppm <1 <1 <1 <1 <![CDATA[Gd2O3]]> ppm <1 <1 <1 <1 <![CDATA[Tb4O7]]> ppm <1 <1 <1 <1 <![CDATA[Dy2O3]]> ppm <1 <1 <1 <1 <![CDATA[Ho2O3]]> ppm <1 <1 <1 <1 <![CDATA[Er2O3]]> ppm <1 <1 <1 <1 <![CDATA[Tm2O3]]> ppm <1 <1 <1 <1 <![CDATA[Yb2O3]]> ppm 5 4 6 5 <![CDATA[Y2O3]]> ppm <1 <1 <1 <1 <![CDATA[Fe2O3]]> ppm <1 <1 <1 <1 <![CDATA[SiO2]]> ppm 7.7 8.0 7.8 8.6 CaO ppm 3.1 2.7 3.0 2.5 <![CDATA[Cl - ]]> ppm 8 7 9 7 <![CDATA[Al2O 3% ]]> ppm 14.1 9.7 7.7 8.4 Table 3 Inspection items unit Comparative Example 1 Comparative Example 2 Comparative Example 3 TREO % 99.42 99.49 99.52 LOI % 0.35 0.37 0.34 <![CDATA[Lu2O3 / TREO]]> % 99.996 99.998 99.997 <![CDATA[La2O3]]> ppm <1 <1 <1 <![CDATA[CeO2]]> ppm <1 <1 <1 <![CDATA[Pr6O 11 ]]> ppm <1 <1 <1 <![CDATA[Nd2O3]]> ppm <1 <1 <1 <![CDATA[Sm2O3]]> ppm <1 <1 <1 <![CDATA[Eu2O3]]> ppm <1 <1 <1 <![CDATA[Gd2O3]]> ppm <1 <1 <1 <![CDATA[Tb4O7]]> ppm <1 <1 <1 <![CDATA[Dy2O3]]> ppm <1 <1 <1 <![CDATA[Ho2O3]]> ppm <1 <1 <1 <![CDATA[Er2O3]]> ppm <1 <1 <1 <![CDATA[Tm2O3]]> ppm <1 <1 <1 <![CDATA[Yb2O3]]> ppm 5 4 4 <![CDATA[Y2O3]]> ppm <1 <1 <1 <![CDATA[Fe2O3]]> ppm <1 <1 <1 <![CDATA[SiO2]]> ppm 7.7 8.0 7.8 CaO ppm 3.1 2.7 3.0 <![CDATA[Cl - ]]> ppm 8 7 9 <![CDATA[Al2O 3% ]]> ppm 14.1 9.7 7.7 From the data analysis of Table 1-2, it can be seen that the physical and chemical analysis of the nano-lutetium oxide powder prepared by the present invention is: TREO>99.6%, Lu2O3 / TREO>99.995%, Yb2O3<10ppm, other single rare earth impurities<1.0ppm, SiO2<10ppm, CaO<5ppm, Al2O3<15ppm, Cl -<10ppm. This indicates that the product is highly pure and has low impurity content. Lutetium oxide with nano-particle size, narrow particle size distribution, low impurity content and good crystallinity has been prepared, which provides a good preparation process for high-performance products.
[0046] Compared with Example 4, the content of Al2O3 and CaO in the product of Comparative Example 1 is significantly higher, indicating that the cyclohexanediaminetetraacetic acid added in the first precipitation process has a good complexing effect on Ca and Al ions, effectively reducing the impurity ions entering the second reverse precipitation process, thereby reducing the impurity ions entering the calcination step.
[0047] Compared with Example 4, the contents of Al2O3 and CaO in the product of Comparative Example 2 are substantially the same as those in Example 4. This indicates that cocamidopropyl betaine has little effect on impurity ions, and mainly affects the size of the finished product (see Table 1).
[0048] Compared with Example 4, the content of Al2O3 and CaO in the product of Comparative Example 3 is higher than that of Example 4. Although there is an impact, it is not particularly obvious.
[0049] The invention adds cyclohexanediaminetetraacetic acid and cocamidopropyl betaine to a precipitant, adjusts a secondary precipitation method, and optimizes process parameters to prepare high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder, thereby providing a better preparation process for the application of nano-lutetium oxide.
[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder, characterized in that: The steps include: (1) Control and adjust Lu in lutetium solution 3+ Ion concentration According to the Lu in the lutetium solution 3+ The concentration is diluted with deionized water or heated to evaporate the water, and the concentration of lutetium chloride is controlled to be 40-45 g / L, and then the pH is adjusted to 4.6-4.8 with sodium hydroxide; 70-75 g of citric acid and 10-15 g of cyclohexanediaminetetraacetic acid are weighed, dissolved and diluted to 1 L with deionized water, and a citric acid aqueous solution with a concentration of 70-75 g / L is prepared; 60-65 g of industrial refined oxalic acid and 1-2 g of cocamidopropyl betaine are weighed, dissolved and diluted to 1 L with deionized water, and a refined oxalic acid aqueous solution with a concentration of 60-65 g / L is prepared; (2) First positive precipitation Pour the lutetium solution into the reactor, heat it to 45-50°C and keep it there, while turning on the stirrer; Add citric acid aqueous solution to the reactor, and add 1L of citric acid aqueous solution in 20 to 25 minutes until the precipitation reaction is complete; continue stirring for 3 to 5 minutes, then stop stirring and let stand for phase separation; (3) Precipitation and dissolution Dissolve the solid phase in step (2) with hydrochloric acid, then add deionized water to dilute it. 3+ Ion concentration is 35-40 g / L; (4) Second anti-precipitation Pour the purified oxalic acid aqueous solution in step (1) into the reactor, heat it to 50-55°C and maintain it, while turning on the stirrer; add the lutetium solution in step (3) into the reactor, and add 1L of the lutetium solution in 30-35 minutes until the precipitation reaction is complete; continue stirring for 3-5 minutes, then stop stirring and let stand for phase separation; (5) Preparation of Lutetium Oxide Finished Product Extract the mother liquor of oxalic acid precipitation in step (4), place the precipitate in a suction filtration device and filter and rinse it with hot water at 50-55°C for 3-5 times, each time for 15-20 minutes; then dehydrate and filter, put the washed lutetium oxalate into a crucible, and burn it in a high-temperature furnace at 850-950°C for more than 2 hours; thus, a lutetium oxide product is obtained; (6) Grinding and screening The lutetium oxide product obtained in step (5) is ground and sieved to obtain high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder.
2. The method for preparing the high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder according to claim 1, characterized in that: The stirring rate in step (2) is 70 to 90 r / min. -1 .
3. The method for preparing the high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder according to claim 1, characterized in that: The stirring rate in step (4) is 40 to 50 r / min. -1 .
4. The method for preparing the high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder according to claim 1, characterized in that: The main components of the lutetium solution are one or more of lutetium chloride and lutetium nitrate; in addition to lutetium, it also contains trace amounts of La, Ce-Yb, and Y rare earth element impurities, and their total content is less than 50ppm.
5. A high-purity, low-chlorine, low-aluminum-calcium nano-lutetium oxide powder, characterized in that: The nano-lutetium oxide powder is prepared by the preparation method according to any one of claims 1 to 4, and by weight, TREO>99.6%, Lu2O3 / TREO>99.995%, Yb2O3<10ppm, other single rare earth impurities<1.0ppm, SiO2<10ppm, CaO<5ppm, Al2O3<15ppm, Cl - <10ppm, powder size is 250~300nm, and the crystal structure is cubic phase.
Citation Information
Patent Citations
Method for precipitation of low-chloride lutetium oxide by chloride system
CN110372027A
Preparation method of low-chlorine lutetium oxide
CN111874937A
Preparation method of low-chloride high-purity lutetium oxide
CN115536053A