Gypsum plastering mortar based on gold tailings and preparation process thereof

By using ingredients such as gold tailings and carbon nanotubes in gypsum plaster mortar to form fluorine-iron groups and loaded perovskite oxides, the problem of lack of effective formaldehyde removal in the existing technology is solved and formaldehyde removal performance is achieved And the improvement of mechanical properties meets the functional needs of building materials.

CN118724522APending Publication Date: 2024-10-01湖南瑞砂环境科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410703650.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology lacks gypsum plastering mortar that can effectively remove formaldehyde and cannot meet the functional needs of building materials.

Method used

Using gypsum plastering mortar based on gold tailings, Fe2O3 is converted into γ-Fe2O3 through high-temperature roasting, and forms fluorine-iron groups with soluble phosphorus and fluorine in phosphogypsum, combined with carbon nanotubes and loaded perovskite oxides , enhance photocatalytic degradation ability and improve formaldehyde removal performance.

Benefits of technology

It achieves good formaldehyde removal performance of gypsum plaster mortar, improves its mechanical properties, reduces the inventory pressure of phosphogypsum, and enhances the functionality of building materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of plastering mortar, in particular to gypsum plastering mortar based on gold tailings and a preparation process thereof.The gypsum plastering mortar is prepared from, by weight, 80-100 parts of cement, 600-650 parts of ardealite, 400-450 parts of gold tailings, 300-350 parts of aggregate, 5-15 parts of admixture and 300-350 parts of water, the mass fraction of iron oxide in the gold tailings is larger than or equal to 8%, and it is tested that the mass fraction of iron oxide in the gold tailings is larger than or equal to 10%. The gypsum plastering mortar prepared by the invention has certain formaldehyde removal capability and excellent mechanical properties, and can reduce the inventory of phosphogypsum and reduce the storage pressure of enterprises.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of plaster mortar, in particular to a gypsum plaster mortar based on gold tailings and a preparation process thereof. Background Art

[0002] my country is a country with abundant gypsum resources, with the largest reserves in the world. A large amount of chemical gypsum is produced every year. Plaster mortar is a general term for a type of mortar that is applied to the building base for leveling or protection. Adding gypsum to plaster mortar can increase the load-bearing capacity of the wall and reduce the possibility of cracking. With the development of the times, the demand for functional building materials is becoming more and more vigorous. At present, there are formaldehyde-removing paints and formaldehyde-removing latex paints, but there are no reports of gypsum plaster mortar that can remove formaldehyde. Summary of the invention

[0003] Purpose of the invention: In view of the above technical problems, the present invention proposes a gypsum plaster mortar based on gold tailings and a preparation process thereof.

[0004] The technical solutions adopted are as follows: A gypsum plaster mortar based on gold tailings comprises the following components in parts by weight: 80-100 parts of cement, 600-650 parts of phosphogypsum, 400-450 parts of gold tailings, 300-350 parts of aggregates, 15-30 parts of carbon nanotubes, 5-15 parts of admixtures, and 300-350 parts of water; The mass fraction of iron oxide in the gold tailings is ≥8%.

[0005] Furthermore, the admixture includes a polycarboxylate water reducer, a retarder and a silicone waterproofing agent.

[0006] Furthermore, the weight ratio of the polycarboxylate water-reducing agent, the retarder and the organosilicon waterproofing agent is 5-10:1:0.1-0.5.

[0007] Furthermore, the retarder is any one or more combinations of citric acid, tartaric acid, borax and sodium hexametaphosphate.

[0008] Furthermore, the carbon nanotubes are loaded with perovskite oxide.

[0009] Furthermore, the perovskite oxide is LaMnO3.

[0010] Furthermore, the preparation method of the carbon nanotubes is as follows: The multi-walled carbon nanotubes are acidified and then dispersed in a polyethylene glycol solution, and water-soluble lanthanum salt and water-soluble manganese salt are added. After stirring evenly, sodium hydroxide solution is added dropwise. After the addition is completed, the mixed solution is transferred to a hydrothermal reactor, sealed and heated to 150-200°C for reaction for 24-48 hours. After the reaction is completed, the precipitate is collected, washed, dried and then calcined.

[0011] Furthermore, the calcination temperature is 800-900° C., and the calcination time is 1-4 hours.

[0012] The present invention also provides a preparation process of gypsum plaster mortar based on gold tailings: The gold tailings are crushed, mixed with phosphogypsum and carbon nanotubes and ball-milled, and then heated to 280-300° C. and roasted for 1-3 hours to obtain a mixed powder. The admixture is added into water and mixed evenly, and then the mixed powder, cement and aggregate are added and stirred evenly.

[0013] Furthermore, the heating rate during calcination is 1-10°C / min.

[0014] Beneficial effects of the present invention: The invention provides a gypsum plaster mortar based on gold tailings. The gold tailings have a high content of Fe2O3. High-temperature roasting can transform Fe2O3 into γ-Fe2O3. Soluble phosphorus and soluble fluorine in phosphogypsum can also be phosphorylated and fluorinated when roasted together with gold tailings to form fluorine-iron groups and phosphorus-iron groups. These groups have strong electron-withdrawing ability, can inhibit the recombination of photogenerated electrons and holes, and are conducive to the generation of hydroxyl free radicals, so that the gypsum plaster mortar has better formaldehyde removal performance. The addition of carbon nanotubes can stimulate more Many photogenerated carriers move to the active sites on the surface of the gold tailings to participate in the catalytic reaction, thereby further improving the photocatalytic degradation activity of the gypsum plaster mortar, and it can also serve as a filler to achieve a certain strengthening and toughening effect. The perovskite oxide loaded on its surface has a certain photocatalytic activity, and can cooperate with carbon nanotubes and γ-Fe2O3 to make the gypsum plaster mortar have better formaldehyde removal performance. After testing, the gypsum plaster mortar prepared by the present invention has a certain formaldehyde removal ability and excellent mechanical properties, and can reduce the inventory of phosphogypsum and alleviate the storage pressure of enterprises. DETAILED DESCRIPTION

[0015] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0016] Cement: PO42.5 Portland cement, Conch; Phosphogypsum: Hunan Julin Chemical Industry Co., Ltd.’s phosphogypsum warehouse; Gold tailings: China Gold Group Hunan Xinrui Mining Co., Ltd., the composition is shown in Table 1 below: Table 1: Chemical composition (mass fraction) / % ; Carbon nanotubes: homemade; Aggregate: Second-zone machine-made sand produced by Lingshou County Shuokai Mineral Products Co., Ltd., with a fine mesh modulus of 2.8, MB≤1.0; Polycarboxylate water reducer: Qingshuichi brand, Wuhan Runxingyuan Technology Co., Ltd.; Citric acid: Zhengzhou Yaobang Chemical Co., Ltd. Silicone waterproofing agent: Jinan Guigang Chemical Co., Ltd. Water: Homemade deionized water. Example 1

[0017] A gypsum plaster mortar based on gold tailings comprises the following components in parts by weight: 90 parts of cement, 650 parts of phosphogypsum, 425 parts of gold tailings, 4 parts of carbon nanotubes, 350 parts of aggregates, 9 parts of polycarboxylate water reducer, 1 part of citric acid, 0.2 parts of silicone waterproofing agent, and 350 parts of water; The preparation method of the above carbon nanotubes is as follows: 10g of commercially available multi-walled carbon nanotubes were placed in a mixed acid of concentrated sulfuric acid and concentrated nitric acid (60ml of concentrated sulfuric acid and 20ml of concentrated nitric acid), stirred in a 50°C water bath for reaction for 30min, then the reaction solution was slowly poured into 4000ml of ice water for dilution, neutralized with 1M sodium hydroxide solution, washed repeatedly until neutral, and finally dried to obtain pre-acidified multi-walled carbon nanotubes, which were then dispersed in 250ml of 10g / L polyethylene glycol solution, 3.24g of lanthanum nitrate and 3.6g of 50% manganese nitrate solution were added, stirred evenly, and 1M sodium hydroxide solution was added dropwise until the pH of the reaction system reached 10, the mixed solution was transferred to a hydrothermal reactor, sealed and heated to 180°C for reaction for 36h, and the precipitate was collected after the reaction was completed, washed thoroughly with deionized water and dried, and then placed in a tubular furnace and calcined at 850°C for 3h.

[0018] Preparation method of the above-mentioned gypsum plaster mortar based on gold tailings: The gold tailings are crushed to a particle size of ≤5μm, then mixed with phosphogypsum and carbon nanotubes and ball-milled for 5 hours and then dried. The resulting mixture is transferred to a tubular furnace, and the tubular furnace is heated to 300°C at a rate of 5°C / min and roasted for 2 hours to obtain a mixed powder. Polycarboxylic acid water reducer, citric acid, and silicone waterproofing agent are added to water and mixed, and then the mixed powder, cement and aggregate are added and stirred for 15 minutes to make it uniform.

[0019] The gypsum plaster mortar prepared in this embodiment was poured into a 40 mm×40 mm×160 mm mold for molding, and then placed on a mortar vibrating table for compaction. After 1 day, the mold was removed and naturally cured for 28 days to obtain a sample, and the compressive and flexural strength of the sample was tested using a microcomputer-controlled universal testing machine; The flexural strength of the specimen was tested using the three-point bending method (support span of 100 mm) with a loading rate of (50 ± 10) N / s, and the compressive strength was found to be 49.3 MPa. After the flexural test, the broken specimen was placed in a fixture with a contact area of ​​40 mm × 40 mm and placed on a testing machine for a compressive strength test at a loading rate of (2400 ± 200) N / s. The flexural test result was 9.6 MPa. Example 2

[0020] A gypsum plaster mortar based on gold tailings comprises the following components in parts by weight: 100 parts of cement, 600 parts of phosphogypsum, 450 parts of gold tailings, 4 parts of carbon nanotubes, 350 parts of aggregates, 9 parts of polycarboxylic acid water reducer, 1 part of citric acid, 0.2 parts of silicone waterproofing agent, and 350 parts of water.

[0021] The preparation method of the carbon nanotubes is the same as that of Example 1; Preparation method of the above-mentioned gypsum plaster mortar based on gold tailings: The gold tailings are crushed to a particle size of ≤5μm, then mixed with phosphogypsum and carbon nanotubes and ball-milled for 5 hours and then dried. The resulting mixture is transferred to a tubular furnace, and the tubular furnace is heated to 300°C at a rate of 5°C / min and roasted for 2 hours to obtain a mixed powder. Polycarboxylic acid water reducer, citric acid, and silicone waterproofing agent are added to water and mixed, and then the mixed powder, cement and aggregate are added and stirred for 15 minutes to make it uniform. Example 3

[0022] A gypsum plaster mortar based on gold tailings comprises the following components in parts by weight: 80 parts of cement, 600 parts of phosphogypsum, 450 parts of gold tailings, 4 parts of carbon nanotubes, 300 parts of aggregates, 9 parts of polycarboxylic acid water reducer, 1 part of citric acid, 0.2 parts of silicone waterproofing agent, and 300 parts of water.

[0023] The preparation method of the carbon nanotubes is the same as that of Example 1; Preparation method of the above-mentioned gypsum plaster mortar based on gold tailings: The gold tailings are crushed to a particle size of ≤5μm, then mixed with phosphogypsum and carbon nanotubes and ball-milled for 5 hours and then dried. The resulting mixture is transferred to a tubular furnace, and the tubular furnace is heated to 300°C at a rate of 5°C / min and roasted for 2 hours to obtain a mixed powder. Polycarboxylic acid water reducer, citric acid, and silicone waterproofing agent are added to water and mixed, and then the mixed powder, cement and aggregate are added and stirred for 15 minutes to make it uniform. Example 4

[0024] A gypsum plaster mortar based on gold tailings comprises the following components in parts by weight: 90 parts of cement, 650 parts of phosphogypsum, 425 parts of gold tailings, 4 parts of carbon nanotubes, 350 parts of aggregates, 9 parts of polycarboxylic acid water reducer, 1 part of citric acid, 0.2 parts of silicone waterproofing agent, and 350 parts of water.

[0025] The preparation method of the carbon nanotubes is the same as that of Example 1; The gold tailings in this embodiment come from Liaoning Jinfeng Gold Mining Co., Ltd., and the composition is shown in Table 2 below: Table 2: Chemical composition (mass fraction) / % ; Preparation method of the above-mentioned gypsum plaster mortar based on gold tailings: The gold tailings are crushed to a particle size of ≤5μm, then mixed with phosphogypsum and carbon nanotubes and ball-milled for 5 hours and then dried. The resulting mixture is transferred to a tubular furnace, and the tubular furnace is heated to 300°C at a rate of 5°C / min and roasted for 2 hours to obtain a mixed powder. Polycarboxylic acid water reducer, citric acid, and silicone waterproofing agent are added to water and mixed, and then the mixed powder, cement and aggregate are added and stirred for 15 minutes to make it uniform. Example 5

[0026] A gypsum plaster mortar based on gold tailings comprises the following components in parts by weight: 90 parts of cement, 650 parts of phosphogypsum, 425 parts of gold tailings, 4 parts of carbon nanotubes, 350 parts of aggregates, 9 parts of polycarboxylic acid water reducer, 1 part of citric acid, 0.2 parts of silicone waterproofing agent, and 350 parts of water.

[0027] The preparation method of the carbon nanotubes is the same as that of Example 1; The gold tailings in this embodiment come from Qianxinan Jinlong Gold Mining Co., Ltd., and the composition is shown in Table 3 below: Table 3: Chemical composition (mass fraction) / % ; Preparation method of the above-mentioned gypsum plaster mortar based on gold tailings: The gold tailings are crushed to a particle size of ≤5μm, then mixed with phosphogypsum and carbon nanotubes and ball-milled for 5 hours and then dried. The resulting mixture is transferred to a tubular furnace, and the tubular furnace is heated to 300°C at a rate of 5°C / min and roasted for 2 hours to obtain a mixed powder. Polycarboxylic acid water reducer, citric acid, and silicone waterproofing agent are added to water and mixed, and then the mixed powder, cement and aggregate are added and stirred for 15 minutes to make it uniform. Example 6

[0028] The method is basically the same as Example 1, except that commercially available multi-walled carbon nanotubes are directly added.

[0029] Comparative Example 1: The method is basically the same as Example 1, except that the gold tailings are replaced by aggregates of the same weight.

[0030] Comparative Example 2: It is basically the same as Example 1, except that no carbon nanotubes are added.

[0031] Preparation method of the above-mentioned gypsum plaster mortar based on gold tailings: The gold tailings are crushed to a particle size of ≤5μm, and then mixed with phosphogypsum and ball-milled for 5h. The resulting mixture is transferred to a tubular furnace, and the tubular furnace is heated to 300℃ at a rate of 5℃ / min and roasted for 2h to obtain a mixed powder. Polycarboxylic acid water reducer, citric acid, and silicone waterproofing agent are added to water and mixed. Then, the mixed powder, cement, and aggregate are added and stirred for 15min to make it uniform.

[0032] Comparative Example 3: It is basically the same as Example 1, except that phosphogypsum is not added.

[0033] Performance testing: The gypsum plaster mortar prepared in Examples 1-5 and Comparative Examples 1-2 was tested for anti-formaldehyde performance, referring to the method in JC / T 1074-2008 "Purification Performance of Indoor Air Purification Functional Coating Materials"; Test conditions: temperature (20±2)℃, relative humidity (50±10)%, cube test chamber: 1m 3 , 50W fluorescent lamp, 10W air fan, take 7 identical test boxes and number them respectively, the inner wall size of the test box is 1250mm×800mm×1000mm, and introduce 10mg / m 3 The gypsum plaster mortar was poured into 500mm×500mm×5mm molds respectively. After drying naturally for 7 days at room temperature, it was placed in a test box for experiment for 24h.

[0034] The test results are shown in Table 4 below: Table 4: ; It can be seen from Table 4 above that the gypsum plaster mortar prepared by the present invention has a certain ability to remove formaldehyde; By comparing Example 1 with Examples 4 and 5, it can be seen that the Fe2O3 content in the gold tailings is positively correlated with the formaldehyde removal performance of the gypsum plaster mortar; By comparing Example 1 with Example 6, it can be seen that LaMnO3 loaded on multi-walled carbon nanotubes plays a positive role in improving the formaldehyde removal performance of gypsum plaster mortar; By comparing Example 1 with Comparative Example 1, it can be seen that the addition of gold tailings plays a greater role in the formaldehyde removal ability of gypsum plaster mortar; By comparing Example 1 with Comparative Examples 2 and 3, it can be seen that the addition of carbon nanotubes and phosphogypsum improves the formaldehyde removal ability of the gypsum plaster mortar.

[0035] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A gypsum plaster mortar based on gold tailings, characterized in that: The composition is calculated by weight: 80-100 parts of cement, 600-650 parts of phosphogypsum, 400-450 parts of gold tailings, 300-350 parts of aggregates, 15-30 parts of carbon nanotubes, 5-15 parts of admixtures, and 300-350 parts of water; The mass fraction of iron oxide in the gold tailings is ≥8%.

2. The gypsum plaster mortar based on gold tailings as claimed in claim 1, characterized in that: The admixtures include polycarboxylate water reducer, retarder and organosilicon waterproofing agent.

3. The gypsum plaster mortar based on gold tailings as claimed in claim 2, characterized in that: The weight ratio of the polycarboxylate water reducer, the retarder and the silicone waterproofing agent is 5-10:1:0.1-0.

5.

4. The gypsum plaster mortar based on gold tailings as claimed in claim 3, characterized in that: The retarder is any one or more combinations of citric acid, tartaric acid, borax and sodium hexametaphosphate.

5. The gypsum plaster mortar based on gold tailings as claimed in claim 1, characterized in that: The carbon nanotubes are loaded with perovskite oxide.

6. The gypsum plaster mortar based on gold tailings as claimed in claim 5, characterized in that: The perovskite oxide is LaMnO3.

7. The gypsum plaster mortar based on gold tailings as claimed in claim 6, characterized in that: The preparation method of the carbon nanotubes is as follows: The multi-walled carbon nanotubes are acidified and then dispersed in a polyethylene glycol solution, and water-soluble lanthanum salt and water-soluble manganese salt are added. After stirring evenly, sodium hydroxide solution is added dropwise. After the addition is completed, the mixed solution is transferred to a hydrothermal reactor, sealed and heated to 150-200°C for reaction for 24-48 hours. After the reaction is completed, the precipitate is collected, washed, dried and then calcined.

8. The gypsum plaster mortar based on gold tailings as claimed in claim 7, characterized in that: The calcination temperature is 800-900°C and the calcination time is 1-4h.

9. A process for preparing gypsum plaster mortar based on gold tailings as claimed in claim 1, characterized in that: The gold tailings are crushed, mixed with phosphogypsum and carbon nanotubes and ball-milled, and then heated to 280-300° C. and roasted for 1-3 hours to obtain a mixed powder. The admixture is added into water and mixed evenly, and then the mixed powder, cement and aggregate are added and stirred evenly.