Photocatalyst water permeable brick surface layer and preparation method thereof
By using water-based epoxy resin emulsion as a carrier in the photocatalyst permeable bricks, nano-titanium dioxide is evenly dispersed through the shell-making and stirring process, which solves the problem of uniformity and strength of the photocatalyst in the surface layer of the permeable bricks, and achieves efficient photocatalytic effects and Water permeability.
Patent Information
- Application Number
- CN202410829054.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-01
AI Technical Summary
During the preparation process of existing photocatalyst permeable bricks, nanoscale titanium dioxide is not easily dispersed, resulting in a reduction in the uniformity and strength of the photocatalyst in the surface layer, affecting the photocatalytic effect and water permeability.
Water-based epoxy resin emulsion is used as the carrier of nano-titanium dioxide, and the white Portland cement and water-based epoxy resin are evenly wrapped on the surface of the aggregate through a shell-making and stirring process to ensure uniform dispersion of nano-titanium dioxide and the maximum light-receiving area.
The photocatalyst titanium dioxide is evenly distributed in the surface layer of the permeable brick, which improves the photocatalytic effect and light transmittance, and at the same time enhances the overall strength and wear resistance of the surface layer.
Smart Images

Figure CN118724533A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road engineering materials, and in particular relates to a photocatalyst water-permeable brick and a preparation method thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] As a photocatalyst material, titanium dioxide has the function of degrading nitrogen oxides and sulfides under ultraviolet light, decomposing a variety of organic substances that are harmful to human health, killing bacteria, and inhibiting the activity of viruses. It is widely used on various types of building surfaces and floors.
[0004] Permeable bricks have a porous structure, and the area exposed to visible light is much larger than that of ordinary impermeable bricks, so they can be used as carriers of photocatalyst materials. At the same time, since permeable bricks have a double-layer structure, the upper layer is the surface layer and the lower layer is the base layer, the preparation methods of the two layers are different and the base layer is basically not exposed to light. Adding photocatalyst materials only to the surface layer can fully guarantee the photocatalytic effect while reducing costs.
[0005] The commonly used photocatalyst titanium dioxide is nanometer-scale and has a large specific surface area and photocatalytic activity, but it also makes it difficult to disperse during the preparation process. The overall light-receiving area of the agglomerated photocatalyst material is significantly reduced, which will also affect the uniformity of the components of the permeable brick surface layer and even reduce the strength of the permeable brick surface layer. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a photocatalyst permeable brick surface layer and a preparation method thereof, using a polymer emulsion as a carrier and a shell-making and stirring process to ensure the uniformity of the raw materials of the permeable brick surface layer, so that the titanium dioxide photocatalyst is evenly distributed on the aggregate surface, ensuring the maximum light receiving area and state of the photocatalyst, and ensuring the photocatalytic effect.
[0007] In order to achieve the above object, the technical solution of the present invention is:
[0008] In the first aspect, a photocatalyst water-permeable brick surface layer is prepared by raw materials including the following components in parts by weight:
[0009] 10-18 parts of white Portland cement, 70-90 parts of 20-40 mesh aggregate, 1.5-2.5 parts of waterborne epoxy resin emulsion, 1.5-2.5 parts of nano titanium dioxide, 0.5-1.5 parts of silica fume and 0.5-1.5 parts of permeable brick reinforcing agent;
[0010] The shell composed of white silicate cement and water-based epoxy resin is wrapped on the surface of the aggregate, and nano titanium dioxide is dispersed in the water-based epoxy resin in the shell.
[0011] Optionally, the white Portland cement is No. 525 white Portland cement.
[0012] Optionally, the aggregate is white sand and / or black sand.
[0013] Optionally, the particle size of the nano titanium dioxide is 3 to 10 nm.
[0014] Optionally, the silica fume is nano-scale silica fume, and the SiO2 content is greater than 90%.
[0015] In a second aspect, the method for preparing the above-mentioned photocatalyst water-permeable brick surface layer comprises the steps of:
[0016] S1. Add 8 to 12 parts of water into the water according to the proportion, stir evenly, and obtain a water-based epoxy resin slurry;
[0017] S2, adding nano titanium dioxide into the water-based epoxy resin slurry several times and stirring evenly to obtain epoxy resin emulsion photocatalyst slurry;
[0018] S3, taking 1 / 3 to 2 / 3 of the total amount of the epoxy resin emulsion photocatalyst slurry, adding it to the aggregate in a stirring state, mixing and stirring, to obtain a first mixture;
[0019] S4, mixing white cement, silica fume and permeable brick reinforcing agent into a dry mix, taking 1 / 3 to 2 / 3 of the total amount of the dry mix, adding it to the first mixture, and stirring until the white cement evenly wraps the aggregate to obtain a second mixture;
[0020] S5, adding the remaining epoxy resin emulsion photocatalyst slurry to the second mixture, stirring evenly, and then adding the remaining white cement, stirring evenly to obtain a third mixture;
[0021] S6, pressing the third mixture into a shape.
[0022] Optionally, in S1, the stirring method is stirring at a medium speed for 30 to 40 seconds.
[0023] Optionally, in S2, all the nano titanium dioxide is added in three times, 1 / 3 of the total amount is added each time, and stirred evenly after each addition, and then added again, and stirred at medium speed for 1 minute after the addition is completed.
[0024] Optionally, in S3, 1 / 2 of the total amount of the epoxy resin emulsion photocatalyst slurry is taken and added to the aggregate in a stirring state, and the aggregate is mixed and stirred for 30 seconds.
[0025] Optionally, in S4, 1 / 2 of the total amount of the dry mix is added to the first mixture and stirred for 1 minute.
[0026] Optionally, in S5, the remaining epoxy resin emulsion photocatalyst slurry is added to the second mixture, stirred for 30 seconds, and then the remaining dry mix is added and stirred for 1 minute.
[0027] In a third aspect, a photocatalyst water-permeable brick comprises a connected surface layer and a base layer, wherein the surface layer is the above-mentioned photocatalyst water-permeable brick surface layer.
[0028] The beneficial effects of the present invention are:
[0029] 1. The present invention uses water-based epoxy resin emulsion as a photocatalyst titanium dioxide carrier, which is evenly wrapped on the aggregate surface after being mixed with white cement, ensuring that the photocatalyst titanium dioxide in the permeable brick surface layer can be evenly dispersed and reach the maximum light receiving area. The water-based epoxy resin emulsion selected by the present invention is fully transparent after hardening, ensuring the maximum light transmittance, further enhancing the working efficiency of the photocatalyst component, and at the same time, the water-based epoxy resin emulsion can also form an interpenetrating and interlocking structural state with cement paste and aggregate after being cured into a film, significantly improving the comprehensive strength and wear resistance of the surface layer material.
[0030] 2. The present invention evenly disperses the photocatalyst titanium dioxide in the water-based epoxy resin emulsion by multiple stirrings, and uses a shell-making stirring process to ensure that the shell formed by the white silicate cement and the water-based epoxy resin is evenly wrapped on the aggregate surface, thereby solving the problem that the photocatalyst titanium dioxide is easy to agglomerate and poorly dispersed during stirring. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0032] Figure 1 It is a structural schematic diagram of Example 1 in the specific implementation manner.
[0033] Among them, 1. aggregate; 2. shell; 3. photocatalyst. DETAILED DESCRIPTION
[0034] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0035] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0036] Example 1
[0037] A photocatalyst water-permeable brick surface layer, the preparation raw materials include the following components in parts by weight:
[0038] 14 parts of white Portland cement, 80 parts of 20-40 mesh aggregate, 2 parts of water-based epoxy resin emulsion, 2 parts of nano titanium dioxide, 1 part of silica fume and 1 part of permeable brick reinforcing agent;
[0039] A shell composed of white silicate cement and water-based epoxy resin is wrapped on the surface of the aggregate, and nano-titanium dioxide is dispersed in the water-based epoxy resin in the shell.
[0040] Among the above ingredients, water-based epoxy resin emulsion is used as a carrier of nano-titanium dioxide to avoid agglomeration of nano-titanium dioxide and is mixed with white silicate cement, such as Figure 1 As shown, a porous shell 2 of a set thickness is formed on the surface of the aggregate 1 of a single particle, which ensures the strength and water permeability of the surface layer. At the same time, by adjusting the ratio of cement and water-based epoxy resin emulsion, the photocatalyst 3 in the shell 2 contacts the outside world through the pores of the porous structure to achieve photocatalytic effect; the transparent epoxy resin improves the light transmittance of the shell 2 and enhances the catalytic efficiency of the photocatalyst 3 component, thereby obtaining a photocatalyst carrier with good catalytic effect.
[0041] White Portland cement is No. 525 white Portland cement, which is a commonly used raw material for permeable brick surface layer.
[0042] The aggregates are white sand and black sand, and the mass ratio of white sand to black sand is 1:1. They can also be replaced by colored quartz sand.
[0043] The water-based epoxy resin emulsion adopts highly transparent bisphenol A epoxy resin.
[0044] The particle size of nano titanium dioxide is 3 to 10 nm and has high photocatalytic activity.
[0045] The silica fume is nano-scale silica fume with SiO2 content greater than 90% and has hydration reaction activity to increase the strength of the surface material.
[0046] The permeable brick reinforcer is a permeable concrete reinforcer. In this embodiment, the commercially available Everbright Ecological SJ1 is used, which can improve the fluidity of the surface material, reduce water consumption, and improve the strength of the surface material.
[0047] The method for preparing the photocatalyst water-permeable brick surface layer in this embodiment comprises the following steps:
[0048] S1. Add the water-based epoxy resin emulsion into water according to the proportion, stir at medium speed for 30 to 40 seconds until uniform, and obtain a water-based epoxy resin slurry;
[0049] S2, adding nano titanium dioxide into the waterborne epoxy resin slurry in 3 times and stirring evenly, adding 1 / 3 of the total amount each time, stirring evenly after each addition, and then adding again, stirring at medium speed for 1 minute after the addition is completed, to obtain epoxy resin emulsion photocatalyst slurry;
[0050] S3, taking 1 / 2 of the total amount of epoxy resin emulsion photocatalyst slurry, adding it to the aggregate in a stirring state, mixing and stirring for 30 seconds to obtain a first mixture;
[0051] S4, mix white cement, silica fume and permeable brick reinforcing agent into a dry mix, take 1 / 2 of the total amount of the dry mix, add it to the first mixture, and stir for 1 minute until the white cement evenly wraps the aggregate to obtain a second mixture;
[0052] S5, adding the remaining epoxy resin emulsion photocatalyst slurry to the second mixture, stirring for 30 seconds until uniform, adding the remaining white cement, stirring for 1 minute until uniform, to obtain a third mixture;
[0053] S6. Load the third mixture into the surface layer hopper of the cement unburned brick machine, add the base material of the permeable brick into the base layer hopper of the cement unburned brick machine, start the machine, and automatically press and shape it.
[0054] Through the above steps, the photocatalyst titanium dioxide is firstly evenly dispersed in the water-based epoxy resin emulsion, and then the shell-making mixing process is used to ensure that the shell formed by the white silicate cement and the water-based epoxy resin is evenly wrapped on the aggregate surface.
[0055] Specifically, the base material of the permeable brick is a common permeable brick base material, and the formula includes: 1 part of 425 ordinary silica cement, 4 parts of 3-5mm uniform coarse aggregate, 1 part of coarse sand, 0.02 parts of permeable brick reinforcing agent, and 0.2 parts of water;
[0056] The process is also the preparation process of ordinary permeable brick base.
[0057] The surface layer thickness of the prepared permeable brick is 5mm, and the base layer thickness is 50mm.
[0058] Comparative Example 1
[0059] 14 parts of white Portland cement, 80 parts of 20-40 mesh aggregate, 2 parts of PVA emulsion, 2 parts of nano titanium dioxide, 1 part of silica fume and 1 part of permeable brick reinforcing agent;
[0060] The preparation method is the same as that in Example 1.
[0061] Comparative Example 2
[0062] This comparative example uses the same preparation raw materials as Example 1, and the difference from Example 1 is that in the preparation method, the water-based epoxy resin emulsion, white cement and water are first mixed into a slurry, and then nano titanium dioxide is added in batches to obtain a shell-making slurry; then the shell-making slurry is added into the aggregate in a stirring state in multiple batches to obtain a permeable brick surface layer.
[0063] Comparative Example 1 uses PVA emulsion or other commonly used emulsions in construction. The film-forming mechanism of ordinary polymer emulsions will hinder the contact between cement and water, and will seriously hinder the cement hydration process. According to actual test tests, ordinary polymer emulsions will significantly reduce the early strength of cement brick permeable brick surface material. The film-forming form of the water-based epoxy resin used in this application is bundle-shaped, and exists in the cement aggregate structure in a rope-like form. The interpenetrating and interlocking structure strengthens the comprehensive strength of the cement aggregate. At the same time, due to its bundle-like form, it does not hinder the contact between cement and water, and does not affect the normal hydration of cement at all. The early strength of cement brick permeable bricks will not be reduced, but will be significantly enhanced.
[0064] In Comparative Example 2, the water-based epoxy resin emulsion cement and aggregate are stirred in advance, and the photocatalyst component is mixed later. Since the photocatalyst component adopts a very fine particle size at the nanometer level in order to achieve the maximum light receiving area, it is difficult to distribute evenly during the post-mixing process, and it is very easy to form a cluster locally, which greatly reduces the light receiving area. At the same time, due to the post-mixing, the nano-scale photocatalyst component is dispersed on the surface of the cement paste, and it is very easy to peel off due to wear during later use. In the present application, the nano-scale photocatalyst component is first stirred in the water-based epoxy resin emulsion, and after stirring evenly, the photocatalyst component is evenly suspended and distributed in the water-based epoxy resin emulsion, which first solves the problem of the easy agglomeration of the nano-scale photocatalyst. After the cement and aggregate are mixed later, the nano-scale photocatalyst component is finally evenly distributed in the cement emulsion slurry, which ensures that the photocatalyst component does not agglomerate, and also reduces the loss of the photocatalyst component caused by the wear of the brick surface in the later stage.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A photocatalyst permeable brick surface layer, characterized in that: The raw materials for preparation include the following components in parts by weight: 10-18 parts of white Portland cement, 70-90 parts of 20-40 mesh aggregate, 1.5-2.5 parts of waterborne epoxy resin emulsion, 1.5-2.5 parts of nano titanium dioxide, 0.5-1.5 parts of silica fume and 0.5-1.5 parts of permeable brick reinforcing agent; The shell formed by the white silicate cement and the water-based epoxy resin is wrapped on the surface of the aggregate, and the nano titanium dioxide is dispersed in the water-based epoxy resin in the shell.
2. The photocatalyst water-permeable brick surface layer as claimed in claim 1, characterized in that: The white silicate cement is No. 525 white silicate cement.
3. The photocatalyst water-permeable brick surface layer as claimed in claim 1, characterized in that: The aggregate is white sand and / or black sand.
4. The photocatalyst water-permeable brick surface layer as claimed in claim 1, characterized in that: The particle size of the nano titanium dioxide is 3-10 nm.
5. The photocatalyst water-permeable brick surface layer as claimed in claim 1, characterized in that: The silica fume is nano-scale silica fume with SiO2 content greater than 90%.
6. The photocatalyst water-permeable brick surface layer as claimed in claim 1, characterized in that: The raw materials for preparation include the following components in parts by weight: 14 parts of white Portland cement, 80 parts of 20-40 mesh aggregate, 2 parts of water-based epoxy resin emulsion, 2 parts of nano titanium dioxide, 1 part of silica fume and 1 part of permeable brick reinforcer.
7. A method for preparing a photocatalyst water-permeable brick surface layer according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Add 8 to 12 parts of water into the water according to the proportion, stir evenly, and obtain a water-based epoxy resin slurry; S2, adding nano titanium dioxide into the water-based epoxy resin slurry several times and stirring evenly to obtain epoxy resin emulsion photocatalyst slurry; S3, taking 1 / 3 to 2 / 3 of the total amount of the epoxy resin emulsion photocatalyst slurry, adding it to the aggregate in a stirring state, mixing and stirring, to obtain a first mixture; S4, mixing white cement, silica fume and permeable brick reinforcing agent into a dry mix, taking 1 / 3 to 2 / 3 of the total amount of the dry mix, adding it to the first mixture, and stirring until the white cement evenly wraps the aggregate to obtain a second mixture; S5, adding the remaining epoxy resin emulsion photocatalyst slurry to the second mixture, stirring evenly, and then adding the remaining white cement, stirring evenly to obtain a third mixture; S6, pressing the third mixture into a shape.
8. The method for preparing the photocatalyst water-permeable brick surface layer according to claim 7, characterized in that: In S1, the stirring method is stirring at a medium speed for 30 to 40 seconds; Optionally, in S2, all the nano titanium dioxide is added in three times, 1 / 3 of the total amount is added each time, and stirred evenly after each addition, and then added again, and stirred at medium speed for 1 minute after the addition is completed; Optionally, in S3, 1 / 2 of the total amount of epoxy resin emulsion photocatalyst slurry is taken and added to the aggregate in a stirring state, and the aggregate is mixed and stirred for 30 seconds; Optionally, in S4, 1 / 2 of the total amount of white cement is added to the first mixture and stirred for 1 minute.
9. The method for preparing the photocatalyst water-permeable brick surface layer according to claim 7, characterized in that: In S5, the remaining epoxy resin emulsion photocatalyst slurry is added to the second mixture, stirred for 30 seconds, and then the remaining white cement is added and stirred for 1 minute.
10. A photocatalyst water-permeable brick, comprising a connected surface layer and a base layer, characterized in that: The surface layer is the photocatalyst water-permeable brick surface layer as described in any one of claims 1-6.