Preparation method of environment-friendly natural gypsum board

By using reinforced auxiliary materials and basalt fibers prepared from natural materials in gypsum boards, the problem of poor durability of gypsum boards in humid environments is solved, the water resistance and compressive strength of gypsum boards are improved, and its stability and service life are enhanced. Environmentally friendly and economical building material effects are achieved.

CN118724549APending Publication Date: 2024-10-01GUIZHOU HUANGGUAN NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311629010.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-01
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing gypsum boards have poor durability in humid environments and are prone to cracking due to moisture, resulting in poor board stability, weakened sound insulation, and reduced flexural and impact strength.

Method used

Using reinforced auxiliary materials prepared from natural materials, combined with gypsum, activated diatomite, boron nitride, basalt fiber and other raw materials, environmentally friendly natural gypsum boards are prepared through pretreatment and reaction steps to increase its wear resistance, toughness and impact resistance. , and improve corrosion resistance through basalt fiber.

Benefits of technology

It improves the water resistance and compressive strength of gypsum board, enhances the stability and service life of the board, has good compactness and impact resistance, and the material is environmentally friendly and low cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, and discloses an environment-friendly natural gypsum board, which is prepared from the following raw materials in parts by weight: 90 to 120 parts of gypsum, 20 to 50 parts of active diatomite, 3 to 8 parts of boron nitride, 8 to 12 parts of white carbon black, 6 to 8 parts of calcium carbonate, 80 to 90 parts of water, 5 to 20 parts of talcum powder, 10 to 35 parts of basalt fiber, 3 to 7 parts of tourmaline powder, 1 to 3 parts of polycarboxylate superplasticizer and 12 to 20 parts of reinforcing auxiliary materials. The preparation method of the reinforced auxiliary material comprises the following steps: step 1, putting the portulaca oleracea into an alkaline solution, heating, stirring, washing to be neutral, and dehydrating and drying for later use; according to the environment-friendly natural gypsum board, the reinforcing auxiliary material prepared from the natural materials is added into the preparation materials of the environment-friendly natural gypsum board, so that the gypsum board finished product has good wear resistance and toughness, stable structure, good durability and certain impact resistance, and the materials are environment-friendly, free of harmful substances and relatively low in application cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a method for preparing an environmentally friendly natural gypsum board. Background Art

[0002] Gypsum board is a material made of building gypsum as the main raw material. It is a building material with light weight, high strength, thin thickness, easy processing, and good sound insulation, heat insulation and fire resistance. It is one of the new lightweight panels that are currently being developed. It has been widely used in interior partitions, wall coverings, ceilings, sound-absorbing panels, ground base panels and various decorative panels in various buildings such as residences, office buildings, shops, hotels and industrial plants.

[0003] The flexural strength and impact resistance of gypsum boards currently on the market mainly depend on the strength of the surface paper. However, when used in an environment with a certain humidity, its durability will be significantly affected. Once the gypsum board is affected by moisture, it is easy to crack at the installation joints, resulting in poor stability of the gypsum board body and reduced sound insulation effect of the board. At the same time, its flexural strength and impact resistance will decrease, affecting the normal use and aesthetics of the gypsum board wall.

[0004] Therefore, the present invention aims to provide a method for preparing an environmentally friendly natural gypsum board to improve the deficiencies of the gypsum board in the prior art. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing an environmentally friendly natural gypsum board, which solves the problem that the durability of the gypsum boards currently on the market will be significantly affected when used in an environment with a certain humidity, resulting in poor stability of the gypsum board body and weakened sound insulation effect of the board.

[0006] To achieve the above purpose, the present invention is implemented through the following technical scheme: an environmentally friendly natural gypsum board, comprising the following raw materials in proportion by weight: 90-120 parts of gypsum, 20-50 parts of activated diatomaceous earth, 3-8 parts of boron nitride, 8-12 parts of white carbon black, 6-8 parts of calcium carbonate, 80-90 parts of water, 5-20 parts of talc, 10-35 parts of basalt fiber, 3-7 parts of tourmaline powder, 1-3 parts of polycarboxylic acid water reducer, and 12-20 parts of reinforcing auxiliary materials.

[0007] Preferably, the preparation method of the strengthening auxiliary material comprises the following steps:

[0008] Step 1: Pretreatment: Place the ramie in an alkaline solution, heat and stir for 20 to 35 minutes, then wash with water until neutral, dehydrate and dry for later use;

[0009] Step 2, material reaction: placing the pretreated ramie in pure water, heating and stirring for 15 to 20 minutes, then adding a reactant to react for 3 to 4 hours, washing the ramie with water until it is neutral after the reaction, soaking it in an ethanol solution for 10 to 15 hours, and drying it to obtain the ramie after the reaction;

[0010] Step 3, powder mixing: grind the ramie after the reaction into powder, then add water candle powder, wood ash and leaf peel powder into the ramie powder, put it in a grinder and grind it for 40 to 50 minutes to finally obtain the strengthening auxiliary material.

[0011] Preferably, in an environmentally friendly natural gypsum board, the ratio of ramie powder, water candle powder, wood ash and coconut peel powder is (1-2): (2-4): (1-3): (1-2).

[0012] Preferably, the reactant is one of ammonium persulfate, potassium persulfate, sodium sulfite and triethanolamine.

[0013] Preferably, the added mass of the reactant is 0.5-0.75% of the total mass of ramie, and the reaction temperature is controlled at 55-65°C.

[0014] Preferably, in step 1, the alkaline solution is a mixture of water and one of sodium hydroxide, potassium hydroxide, calcium hydroxide and barium hydroxide, and the concentration of the alkaline solution is 1.00 to 1.25 mol / L.

[0015] Preferably, in step 1, the heating temperature range of the alkaline solution is controlled at 55-65°C.

[0016] A method for preparing an environmentally friendly natural gypsum board comprises the following preparation steps:

[0017] S1, adding gypsum to a dryer for preliminary drying treatment, and then after calcination and cooling, adding activated diatomaceous earth, white carbon black, calcium carbonate, water, talcum powder, polycarboxylate water reducer, basalt fiber, and tourmaline powder to the gypsum for mixing to obtain a mixed slurry 1;

[0018] S2, sequentially placing boron nitride, strengthening auxiliary materials and water into a stirring device for mixing and stirring to obtain a mixed slurry 2;

[0019] S3, feeding the mixed slurry obtained in step S2 into an extruder for extrusion to obtain granules;

[0020] S4, preliminarily mixing the mixed slurry obtained in step S1 with the granules obtained in step S2, then injecting the mixture into a plate-type forming machine for extrusion molding, and drying and solidifying to obtain a gypsum base plate;

[0021] S5. Cover the surface of the gypsum base plate obtained in step S4 with an outer layer of paper by means of an adhesive, and obtain an environmentally friendly natural gypsum board product after cutting and trimming.

[0022] Preferably, in step 1, the drying environment temperature of the gypsum is controlled at 100-150° C., and the drying time is maintained at 8-15 hours.

[0023] Preferably, in step S1, the gypsum calcination temperature is controlled at 170-240° C., and the calcination time is controlled at 15-28 hours.

[0024] The present invention provides a method for preparing an environmentally friendly natural gypsum board, which has the following beneficial effects:

[0025] 1. The present invention adds reinforcing auxiliary materials made of natural materials to the preparation materials of environmentally friendly natural gypsum boards, so that the finished gypsum boards have good wear resistance and toughness, and at the same time the density is significantly improved, the structure is stable, the durability is good, and it has a certain impact resistance. In addition, the materials are environmentally friendly, free of harmful substances, and have a low application cost.

[0026] 2. The present invention uses basalt fiber in the preparation raw materials of the present invention, which is used to cooperate with other raw materials to assist in improving the corrosion resistance of the gypsum board, so that the gypsum board has good water resistance in a high humidity environment, improves the service life of the gypsum board, and at the same time is better in compressive strength than conventional gypsum board products. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0028] The invention provides a method for preparing an environment-friendly natural gypsum board, wherein the main raw materials of the environment-friendly natural gypsum board include: gypsum, activated diatomaceous earth, boron nitride, outer paper, white carbon black, calcium carbonate, water, talcum powder, basalt fiber, tourmaline powder, polycarboxylic acid water reducer, and strengthening auxiliary materials.

[0029] Furthermore, in the raw materials for preparing the environmentally friendly natural gypsum board, the reinforcing auxiliary material is prepared by the following method steps:

[0030] Step 1: Pretreatment: Place the ramie in an alkaline solution, heat and stir for 20 to 35 minutes, then wash with water until neutral, dehydrate and dry for later use;

[0031] Step 2, material reaction: placing the pretreated ramie in pure water, adding a reactant after heating and stirring, reacting for 3 to 4 hours under a certain temperature environment, washing the ramie with water until it is neutral after the reaction, soaking it in an ethanol solution for 10 to 15 hours, and drying it to obtain the ramie after the reaction;

[0032] Step 3, powder mixing: grind the ramie after the reaction into powder, then add water candle powder, wood ash and leaf peel powder into the ramie powder, put it in a grinder and grind it to obtain the strengthening auxiliary material.

[0033] In this environmentally friendly natural gypsum board, by adding reinforcing auxiliary materials made from natural materials, the finished gypsum board has good wear resistance and toughness, and the density is significantly improved. The plant fiber provides the required strength for the gypsum board, and the structure is stable, durable, and has a certain impact resistance.

[0034] The basalt fiber is used in the preparation raw materials of the present invention to cooperate with other raw materials to assist in improving the corrosion resistance of the gypsum board, so that the gypsum board has good water resistance in a high humidity environment, improves the service life of the gypsum board, and is better in compressive strength than conventional gypsum board products.

[0035] The technical scheme and technical effects of the present invention are further described below in conjunction with specific embodiments.

[0036] Embodiment 1:

[0037] An embodiment of the present invention provides a method for preparing an environmentally friendly natural gypsum board, wherein the environmentally friendly natural gypsum board comprises the following raw materials in proportion by weight: 90 parts of gypsum, 20 parts of activated diatomaceous earth, 3 parts of boron nitride, 8 parts of white carbon black, 6 parts of calcium carbonate, 80 parts of water, 5 parts of talc, 10 parts of basalt fiber, 3 parts of tourmaline powder, 1 part of polycarboxylic acid water reducer, and 12 parts of reinforcing auxiliary materials.

[0038] In this embodiment, the strengthening auxiliary material is prepared by the following method:

[0039] Step 1, pretreatment operation: put the ramie in an alkaline solution, heat and stir for 20 minutes, then wash with water until neutral, dehydrate and dry for use. In this step, the ratio of ramie powder, water candle powder, plant ash and coconut peel powder is 1:2:1:1, wherein the alkaline solution is a mixture of barium hydroxide and water, the concentration is 1.25 mol / L, and the heating temperature is controlled at 65°C;

[0040] Step 2, material reaction: put the pretreated ramie into pure water, heat and stir for 20 minutes, then add the reactant to react for 3 hours, after the reaction is completed, wash the ramie with water until it is neutral, soak it in an ethanol solution for 10 hours, and dry it to obtain the ramie after reaction treatment. In this step, the reactant is ammonium persulfate, and its added mass is 0.5-0.75% of the total mass of the ramie, and the reaction temperature is controlled at 55-65°C;

[0041] Step 3, powder mixing: grind the ramie after the reaction into powder, then add water candle powder, wood ash and leaf peel powder into the ramie powder, put it in a grinder and grind it for 40 minutes to finally obtain the reinforced auxiliary material.

[0042] Furthermore, in this embodiment, the method for preparing the environmentally friendly natural gypsum board includes the following preparation steps:

[0043] S1, adding gypsum to a dryer for preliminary drying treatment, and then after calcination and cooling, adding activated diatomaceous earth, white carbon black, calcium carbonate, water, talcum powder, polycarboxylate water reducer, basalt fiber, and tourmaline powder to the gypsum for mixing to obtain a mixed slurry 1. In this step, the drying environment temperature of the gypsum is controlled at 150° C., the drying time is maintained at 15 hours, and the gypsum calcination temperature is controlled at 220° C., and the calcination time is controlled at 15 hours;

[0044] S2, sequentially placing boron nitride, strengthening auxiliary materials and water into a stirring device for mixing and stirring to obtain a mixed slurry 2;

[0045] S3, feeding the mixed slurry obtained in step S2 into an extruder for extrusion to obtain granules;

[0046] S4, preliminarily mixing the mixed slurry obtained in step S1 with the granules obtained in step S2, then injecting the mixture into a plate-type forming machine for extrusion molding, and drying and solidifying to obtain a gypsum base plate;

[0047] S5. Cover the surface of the gypsum base plate obtained in step S4 with an outer layer of paper by means of an adhesive, and obtain an environmentally friendly natural gypsum board product after cutting and trimming.

[0048] The comprehensive performance parameters of the environmentally friendly natural gypsum board product prepared in this embodiment are shown in Table 2.

[0049] Embodiment 2:

[0050] An embodiment of the present invention provides a method for preparing an environmentally friendly natural gypsum board, wherein the environmentally friendly natural gypsum board comprises the following raw materials in proportion by weight: 90 parts of gypsum, 20 parts of activated diatomaceous earth, 4 parts of boron nitride, 8 parts of white carbon black, 6 parts of calcium carbonate, 80 parts of water, 5 parts of talc, 10 parts of basalt fiber, 3 parts of tourmaline powder, 1 part of polycarboxylic acid water reducer, and 14 parts of reinforcing auxiliary materials.

[0051] In this embodiment, the preparation method of the reinforcing auxiliary material and the preparation method of the environmentally friendly natural gypsum board finished product are consistent with those in Example 1. The comprehensive performance parameters of the environmentally friendly natural gypsum board finished product prepared by this embodiment are shown in Table 2.

[0052] Embodiment 3:

[0053] An embodiment of the present invention provides a method for preparing an environmentally friendly natural gypsum board, wherein the environmentally friendly natural gypsum board comprises the following raw materials in proportion by weight: 90 parts of gypsum, 20 parts of activated diatomaceous earth, 5 parts of boron nitride, 8 parts of white carbon black, 6 parts of calcium carbonate, 80 parts of water, 5 parts of talc, 10 parts of basalt fiber, 3 parts of tourmaline powder, 1 part of polycarboxylic acid water reducer, and 16 parts of reinforcing auxiliary materials.

[0054] In this embodiment, the preparation method of the reinforcing auxiliary material and the preparation method of the environmentally friendly natural gypsum board finished product are consistent with those in Example 1. The comprehensive performance parameters of the environmentally friendly natural gypsum board finished product prepared by this embodiment are shown in Table 2.

[0055] Embodiment 4:

[0056] An embodiment of the present invention provides a method for preparing an environmentally friendly natural gypsum board, wherein the environmentally friendly natural gypsum board comprises the following raw materials in proportion by weight: 90 parts of gypsum, 20 parts of activated diatomaceous earth, 6 parts of boron nitride, 8 parts of white carbon black, 6 parts of calcium carbonate, 80 parts of water, 5 parts of talc, 10 parts of basalt fiber, 3 parts of tourmaline powder, 1 part of polycarboxylic acid water reducer, and 18 parts of reinforcing auxiliary materials.

[0057] In this embodiment, the preparation method of the reinforcing auxiliary material and the preparation method of the environmentally friendly natural gypsum board finished product are consistent with those in Example 1. The comprehensive performance parameters of the environmentally friendly natural gypsum board finished product prepared by this embodiment are shown in Table 2.

[0058] Embodiment 5:

[0059] An embodiment of the present invention provides a method for preparing an environmentally friendly natural gypsum board, wherein the environmentally friendly natural gypsum board comprises the following raw materials in proportion by weight: 90 parts of gypsum, 20 parts of activated diatomaceous earth, 7 parts of boron nitride, 8 parts of white carbon black, 6 parts of calcium carbonate, 80 parts of water, 5 parts of talc, 10 parts of basalt fiber, 3 parts of tourmaline powder, 1 part of polycarboxylic acid water reducer, and 20 parts of reinforcing auxiliary materials.

[0060] In this embodiment, the preparation method of the reinforcing auxiliary material and the preparation method of the environmentally friendly natural gypsum board finished product are consistent with those in Example 1. The comprehensive performance parameters of the environmentally friendly natural gypsum board finished product prepared by this embodiment are shown in Table 2.

[0061] Comparative Example 1:

[0062] This comparative example provides a method for preparing an environmentally friendly natural gypsum board, wherein the environmentally friendly natural gypsum board comprises the following raw materials in proportion by weight: 90 parts of gypsum, 25 parts of activated diatomaceous earth, 10 parts of white carbon black, 6 parts of calcium carbonate, 80 parts of water, 5 parts of talc, 10 parts of basalt fiber, 3 parts of tourmaline powder, and 1 part of polycarboxylic acid water reducer.

[0063] In this comparative example, compared with Examples 1-5, the preparation method remains the same, the difference is that the types of raw materials added are changed, and boron nitride and strengthening auxiliary materials are removed.

[0064] Comparative Example 2:

[0065] This comparative example provides a gypsum board, the main raw materials of which include: 30 parts of desulfurized gypsum, 35 parts of phosphogypsum, 15 parts of talcum powder, 50 parts of water, and 8 parts of binder;

[0066] The binder consists of the following ingredients: 10 parts of epoxy resin, 10 parts of acrylic acid water-based adhesive, 15 parts of kaolin, and 10 parts of modified starch.

[0067] Table 1: Parameter setting table of internal strengthening auxiliary materials and boron nitride addition of gypsum board in Examples 1-5

[0068] Serial number Example 1 Example 2 Example 3 Example 4 Example 5 Strengthening excipients 12 servings 14 servings 16 servings 18 servings 20 servings Boron Nitride 3 servings 4 servings 5 servings 6 servings 7 servings

[0069] Auxiliary experiments:

[0070] The paper-faced gypsum board of the present invention and the commercially available gypsum board were used for the wall of the bathroom. The same gypsum board with the same area was used for the upper and lower parts of the same wall. The air humidity was maintained at 90%. After 3 months of testing, the results are shown in Table 2 below.

[0071] Table 2: Comprehensive performance data of environmentally friendly natural gypsum board

[0072] Serial number Water loss rate / % Compressive strength / MPa Is there any crack at the seam? Example 1 1.8 289 no Example 2 1.6 295 no Example 3 1.3 303 no Example 4 0.9 310 no Example 5 0.8 317 no Comparative Example 1 4.7 216 yes Comparative Example 2 8.9 183 yes

[0073] From the data in Table 1 combined with Table 2, the finished gypsum board prepared by the embodiment of the present invention was tested for 3 months under the same humidity conditions, and no cracking occurred at the installation joints of the gypsum board, while the comparative examples 1-2 involved in the experiment all had cracking problems. At the same time, the gypsum board products of the embodiment of the present invention were superior to the two gypsum board products improved by the comparative examples in terms of water loss resistance and compressive strength, which shows that the environmentally friendly natural gypsum board prepared by the present invention has excellent performance and can achieve better results in construction applications.

[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An environmentally friendly natural gypsum board, It is characterized in that The invention comprises the following raw materials in proportion by weight: 90-120 parts of gypsum, 20-50 parts of activated diatomaceous earth, 3-8 parts of boron nitride, 8-12 parts of white carbon black, 6-8 parts of calcium carbonate, 80-90 parts of water, 5-20 parts of talc, 10-35 parts of basalt fiber, 3-7 parts of tourmaline powder, 1-3 parts of polycarboxylic acid water reducer and 12-20 parts of reinforcing auxiliary materials.

2. The environmentally friendly natural gypsum board according to claim 1, It is characterized in that The preparation method of the strengthening auxiliary material comprises the following steps: Step 1: Pretreatment: Place the ramie in an alkaline solution, heat and stir for 20 to 35 minutes, then wash with water until neutral, dehydrate and dry for later use; Step 2, material reaction: placing the pretreated ramie in pure water, heating and stirring for 15 to 20 minutes, then adding a reactant to react for 3 to 4 hours, washing the ramie with water until it is neutral after the reaction, soaking it in an ethanol solution for 10 to 15 hours, and drying it to obtain the ramie after the reaction; Step 3, powder mixing: grind the ramie after the reaction into powder, then add water candle powder, wood ash and leaf peel powder into the ramie powder, put it in a grinder and grind it for 40 to 50 minutes to finally obtain the strengthening auxiliary material.

3. The environmentally friendly natural gypsum board according to claim 2, It is characterized in that According to the environmentally friendly natural gypsum board of claim 2, the ratio of ramie powder, water candle powder, wood ash and coconut peel powder is (1-2): (2-4): (1-3): (1-2).

4. The environmentally friendly natural gypsum board according to claim 2, It is characterized in that The reactant is one of ammonium persulfate, potassium persulfate, sodium sulfite and triethanolamine.

5. The environmentally friendly natural gypsum board according to claim 2, It is characterized in that The added mass of the reactant is 0.5-0.75% of the total mass of the ramie, and the reaction temperature is controlled at 55-65°C.

6. The environmentally friendly natural gypsum board according to claim 2, It is characterized in that In the step 1, the alkaline solution is a mixture of water and one of sodium hydroxide, potassium hydroxide, calcium hydroxide, and barium hydroxide, and the concentration of the alkaline solution is 1.00 to 1.25 mol / L.

7. The environmentally friendly natural gypsum board according to claim 2, It is characterized in that In the step 1, the heating temperature range of the alkaline solution is controlled at 55-65°C.

8. A method for preparing an environmentally friendly natural gypsum board, It is characterized in that An environmentally friendly natural gypsum board as claimed in any one of claims 1 to 3 comprises the following preparation steps: S1, adding gypsum to a dryer for preliminary drying treatment, and then after calcination and cooling, adding activated diatomaceous earth, white carbon black, calcium carbonate, water, talcum powder, polycarboxylate water reducer, basalt fiber, and tourmaline powder to the gypsum for mixing to obtain a mixed slurry 1; S2, sequentially placing boron nitride, strengthening auxiliary materials and water into a stirring device for mixing and stirring to obtain a mixed slurry 2; S3, feeding the mixed slurry obtained in step S2 into an extruder for extrusion to obtain granules; S4, preliminarily mixing the mixed slurry obtained in step S1 with the granules obtained in step S2, then injecting the mixture into a plate-type forming machine for extrusion molding, and drying and solidifying to obtain a gypsum base plate; S5. Cover the surface of the gypsum base plate obtained in step S4 with an outer layer of paper by means of an adhesive, and obtain an environmentally friendly natural gypsum board product after cutting and trimming.

9. A method for preparing an environmentally friendly natural gypsum board according to claim 8, It is characterized in that In the step 1, the drying environment temperature of the gypsum is controlled at 100-150° C., and the drying time is maintained at 8-15 hours.

10. The method for preparing an environmentally friendly natural gypsum board according to claim 8, It is characterized in that In the step S1, the gypsum calcination temperature is controlled at 170-240° C., and the calcination time is controlled at 15-28 hours.

Citation Information

Cited By

  • Anti-bending gypsum plaster board and preparation method thereof

    CN120025148A