Geopolymer combined silicon carbide refractory material and preparation method thereof

By using geopolymer binders, the core-shell structure of silicon carbide refractory materials is formed, which solves the problems of creep and oxidation of existing silicon carbide refractory materials at high temperatures, improves the density and oxidation resistance of the material, and reduces production costs. and energy consumption.

CN118724600AActive Publication Date: 2024-10-01TAIZHOU WANGXIN REFRACTORIES CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410782843.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Existing silicon carbide refractory materials have problems such as creep, high production costs, high energy consumption and surface oxidation under high temperature conditions, resulting in reduced performance.

Method used

Using geopolymer as a binding agent, a sol is formed by mechanically mixing aluminum silicate powder, phosphoric acid activator and water, stirred evenly with silicon carbide, pressed and sintered at low temperature in an air atmosphere to form a uniform core-shell structure to improve density. and antioxidant properties.

Benefits of technology

It effectively improves the density and strength of the material, reduces production costs, avoids the formation of secondary pores, enhances oxidation resistance and thermal shock stability, and achieves low-temperature densification sintering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724600A_ABST
    Figure CN118724600A_ABST
Patent Text Reader

Abstract

The invention discloses a geopolymer combined silicon carbide refractory material and a preparation method thereof. The refractory material is prepared from the following substances in percentage by weight: 70 to 90 weight percent of silicon carbide, 7 to 21 weight percent of aluminum silicate powder, 1 to 3 weight percent of phosphoric acid exciting agent and 2 to 6 weight percent of water. The preparation method has the beneficial effects that the preparation method has the characteristics of low cost, simple process, feasibility, high efficiency, low carbon, greenness and no pollution, and the prepared geopolymer combined silicon carbide refractory material is uniform in pore distribution, excellent in mechanical property, excellent in oxidation resistance and excellent in thermal shock resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon carbide refractory materials, in particular to a geopolymer-bonded silicon carbide refractory material and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC) material has excellent properties such as high mechanical strength, low thermal expansion coefficient, strong thermal shock resistance and chemical corrosion resistance. It is widely used in metallurgy, energy and chemical industries. SiC has strong covalent bond characteristics and is difficult to sinter. Usually, a second bonding phase is added to obtain a dense silicon carbide sintered body. The second phase of SiC refractory materials includes clay, silica, mullite, silicon nitride, silicon oxynitride and sialon. According to the type of bonding phase, SiC refractory products can be divided into oxide-bonded silicon carbide, nitride-bonded silicon carbide and self-bonded silicon carbide. However, the existing SiC refractory products have the following significant problems: ① The production process of oxide-bonded silicon carbide refractory materials is simple, but the oxide is prone to creep under high temperature conditions and cannot be used at high temperatures; ② The use temperature of nitride-bonded silicon carbide refractory materials is high, but the process is complicated, the production cost is high, and there is a thermal mismatch between nitride and silicon carbide; ③ The synthesis temperature of self-bonded silicon carbide refractory materials is high, the production cost is high, the energy consumption is large, and the presence of residual carbon and free silicon makes the high temperature performance worse;

[0003] When sintered in an unprotected atmosphere or used at high temperatures, the surface of nitride-bonded silicon carbide and self-bonded silicon carbide refractory materials is easily oxidized, and it is inevitable that amorphous silicon dioxide or quartz will remain in the neck, which seriously affects the performance of silicon carbide products. Oxide-bonded silicon carbide can be sintered in an oxidizing atmosphere at normal pressure, and its production cost is relatively low. It is currently the most important bonding method for silicon carbide products. The preparation of SiC refractory products adopts coarse, medium and fine graded ingredients, with silicon carbide and bonding phase as raw materials. In order to ensure sufficient green body strength, a temporary binder is selected, the raw materials are pressed into shape, and then fired at 1200-1400℃. Commonly used binders include organic binders such as pulp waste liquid, dextrin, resin and polyvinyl alcohol. However, the loss of such binders during the firing process will produce secondary pores or voids in the material structure, resulting in a decrease in mechanical strength, thermal conductivity, corrosion resistance and wear resistance. Summary of the invention

[0004] The purpose of the present invention is to solve the above problems and to design a geopolymer-bonded silicon carbide refractory material and a preparation method thereof.

[0005] To achieve the above-mentioned purpose, the technical solution of the present invention is a geopolymer-bonded silicon carbide refractory material, which is composed of the following substances in weight percentage: 70-90wt% of silicon carbide, 7-21wt% of aluminum silicate powder, 1-3wt% of phosphoric acid activator and 2-6wt% of water as raw materials.

[0006] A method for preparing a geopolymer-bonded silicon carbide refractory material comprises the following steps:

[0007] Step 1: first mechanically mix aluminum silicate powder, phosphoric acid activator and water to obtain a geopolymer sol;

[0008] Step 2: Stir the sol and silicon carbide evenly; press and form under 80-200 MPa, dry at 110°C for 48 hours, heat to 1200-1400°C at a rate of 2-10°C / min in air atmosphere, keep warm for 2-5 hours, and cool to room temperature with the furnace;

[0009] Step 3: Prepare geopolymer-bonded silicon carbide refractory material.

[0010] As a further supplement to the technical solution, the SiC content in the silicon carbide is ≥98wt% and the particle size is ≤3mm.

[0011] As a further supplement to the technical solution, the aluminum silicate powder is a combination of one or more of pyrophyllite, kaolin, sillimanite, vermiculite and mica.

[0012] As a further supplement to the technical solution, the phosphoric acid activator is a combination of one or more of orthophosphoric acid, phosphorous acid, metaphosphoric acid and polyphosphoric acid.

[0013] The beneficial effect lies in that the present invention adopts geopolymer as a forming binder for silicon carbide refractory materials. Geopolymer is a kind of inorganic polymer sol with a three-dimensional network structure of silicon oxygen tetrahedron and aluminum oxygen tetrahedron, which can avoid the secondary pores or pores generated by traditional organic binders during the material firing process, and effectively improve the density and strength of the product; the present invention adopts natural aluminum silicate mineral as a raw material to obtain the geopolymer binder, and forms high-temperature ceramic binding phases such as mullite, calcium feldspar, cordierite and olivine in situ under calcination conditions. A small amount of alkali metal impurities in the mineral raw materials can reduce the formation temperature of the ceramic binding phase and realize the low-temperature densification sintering of silicon carbide refractory materials; the present invention forms a coating on the surface of silicon carbide particles through the geopolymer sol binder, and polymerization occurs during the drying process to form a gel, which provides initial strength for the green embryo, and the ceramic binding phase is generated in situ on the surface of silicon carbide during the firing process, forming a uniform coating to form a core-shell structure (silicon carbide as the core and the ceramic binding phase as the shell) ), while providing bonding strength for the material, it can avoid the contact between silicon carbide and oxygen-containing gas, realize the sintering of silicon carbide refractory materials in air atmosphere, and improve the oxidation resistance of the materials; the aluminum silicate raw materials used in the present invention include pyrophyllite, kaolin, sillimanite, vermiculite and mica, all of which are commonly used raw materials in the ceramic industry. The raw materials are easy to obtain and low in price, which can reduce the preparation cost of the materials; the geopolymer combined with silicon carbide refractory material prepared by the present invention has been tested: the apparent porosity is 10-20%; the room temperature flexural strength is 20-50MPa; the compressive strength is 150-300MPa; the residual flexural strength retention rate (thermal shock stability) is 50-90% (1100℃ water cooling 3 times); and it has good corrosion resistance and oxidation resistance; the present invention has the characteristics of low cost, simple process, feasible and efficient, low-carbon, green and pollution-free, and the prepared geopolymer combined with silicon carbide refractory material has uniform pore distribution, excellent mechanical properties, excellent oxidation resistance and excellent thermal shock resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is an XRD spectrum of a geopolymer combined with silicon carbide refractory material prepared by the present invention;

[0015] Figure 2 This is a microstructure diagram of a geopolymer-bonded silicon carbide refractory material prepared in the present invention. DETAILED DESCRIPTION

[0016] In order to make the technical solution more clear to those skilled in the art, the technical solution of the present invention will be described in detail below in conjunction with embodiments:

[0017] To avoid repetition, the raw materials involved in this specific implementation are first described as follows, and no further details are given in the examples: the SiC content in the silicon carbide is ≥98wt%, and the particle size is ≤3mm; the aluminum silicate powder is one or more of pyrophyllite, kaolin, sillimanite, vermiculite and mica; the phosphoric acid activator is one or more of orthophosphoric acid, phosphorous acid, metaphosphoric acid and polyphosphoric acid; the implementation scheme will be described in detail below:

[0018] Example 1

[0019] A preparation method of a geopolymer-bonded silicon carbide refractory material comprises the following steps: using 70-75wt% of silicon carbide, 17-21wt% of aluminum silicate powder, 1-2wt% of a phosphoric acid activator and 5-6wt% of water as raw materials; firstly mechanically mixing the aluminum silicate powder, the phosphoric acid activator and the water to obtain a geopolymer sol; then uniformly stirring the sol and the silicon carbide; pressing and molding under the condition of 80-100MPa, then drying at 110°C for 48 hours, heating to 1200-1300°C at a rate of 2-5°C / min in an air atmosphere, keeping the temperature for 2-3 hours, and cooling to room temperature with the furnace to obtain the geopolymer-bonded silicon carbide refractory material.

[0020] In this embodiment, the aluminum silicate powder is 8-9wt% pyrophyllite and 9-12wt% kaolin powder; the phosphoric acid is 0.5-1wt% orthophosphoric acid and 0.5-1wt% phosphorous acid.

[0021] The geopolymer combined with silicon carbide refractory prepared by the present invention has been tested to have an apparent porosity of 15-20%, a room temperature flexural strength of 20-30 MPa, a compressive strength of 150-200 MPa, and a residual flexural strength retention rate (thermal shock stability) of 50-60% (water-cooled at 1100°C for 3 times).

[0022] Example 2

[0023] A preparation method of a geopolymer-bonded silicon carbide refractory material comprises the following steps: using 75-80 wt% of silicon carbide, 15-19 wt% of aluminum silicate powder, 1-2 wt% of a phosphoric acid activator and 4-6 wt% of water as raw materials; firstly mechanically mixing the aluminum silicate powder, the phosphoric acid activator and the water to obtain a geopolymer sol; then uniformly stirring the sol and the silicon carbide; pressing and molding under the condition of 100-150 MPa, then drying at 110 DEG C for 48 hours, heating to 1200-1300 DEG C at a rate of 2-5 DEG C / min in an air atmosphere, keeping the temperature for 2-3 hours, and cooling to room temperature with the furnace to obtain the geopolymer-bonded silicon carbide refractory material. Figure 1 The XRD spectrum of the product in this embodiment shows that the phase composition is silicon carbide and cordierite.

[0024] In this embodiment, the aluminum silicate powder is 2-4wt% kaolin, 4-5wt% sillimanite and 9-10wt% vermiculite powder; the phosphoric acid is 0.5-1wt% orthophosphoric acid, 0.25-0.5wt% phosphorous acid and 0.25-0.5wt% metaphosphoric acid.

[0025] The geopolymer combined with silicon carbide refractory prepared by the present invention has been tested to have an apparent porosity of 10-15%, a room temperature flexural strength of 30-40 MPa, a compressive strength of 200-250 MPa, and a residual flexural strength retention rate (thermal shock stability) of 60-70% (water-cooled at 1100°C for 3 times).

[0026] Example 3

[0027] A preparation method of a geopolymer-bonded silicon carbide refractory material comprises the following steps: using 80-85wt% of silicon carbide, 9-15wt% of aluminum silicate powder, 2-3wt% of a phosphoric acid activator and 3-4wt% of water as raw materials; firstly mechanically mixing the aluminum silicate powder, the phosphoric acid activator and the water to obtain a geopolymer sol; then uniformly stirring the sol and the silicon carbide; pressing and molding under the condition of 100-150MPa, then drying at 110°C for 48 hours, heating to 1300-1400°C at a rate of 2-5°C / min in an air atmosphere, keeping the temperature for 3-5 hours, and cooling to room temperature with the furnace to obtain the geopolymer-bonded silicon carbide refractory material. Figure 1 The XRD spectrum of the product in this embodiment shows that the phase composition is silicon carbide and cordierite.

[0028] In this embodiment, the aluminum silicate powder is 2-3wt% kaolin, 2-3wt% sillimanite, 4-7wt% vermiculite and 1-2wt% mica powder; the phosphoric acid is 1-1.5wt% orthophosphoric acid, 0.5-0.75wt% phosphorous acid and 0.5-0.75wt% metaphosphoric acid.

[0029] The geopolymer combined with silicon carbide refractory prepared by the present invention is tested: the apparent porosity is 10-15%; the room temperature flexural strength is 30-40MPa; the compressive strength is 200-250MPa; the residual flexural strength retention rate (thermal shock stability) is 70-80% (1100°C water cooling 3 times);

[0030] Example 4

[0031] A preparation method of a geopolymer-bonded silicon carbide refractory material comprises the following steps: using 85-90 wt% of silicon carbide, 7-10 wt% of pyrophyllite, kaolin, sillimanite, vermiculite and mica powder, 2-3 wt% of orthophosphoric acid, phosphorous acid, metaphosphoric acid and polyphosphoric acid activators and 2-3 wt% of water as raw materials; firstly mechanically mixing aluminum silicate powder, phosphoric acid activator and water to obtain geopolymer sol; then stirring the sol and silicon carbide uniformly; pressing and molding under the condition of 150-200 MPa, then drying at 110 DEG C for 48 hours, heating to 1300-1400 DEG C at a rate of 5-10 DEG C / min in an air atmosphere, keeping the temperature for 3-5 hours, cooling to room temperature with the furnace, and obtaining the geopolymer-bonded silicon carbide refractory material.

[0032] In this embodiment: the aluminum silicate powder is 1.5-2wt% pyrophyllite, 0.5-1wt% kaolin, 1.5-2wt% sillimanite, 3-4wt% vermiculite and 0.5-1wt% mica powder; the phosphoric acid is 1-1.25wt% orthophosphoric acid, 0.25-0.5wt% phosphorous acid, 0.25-0.5wt% metaphosphoric acid and 0.5-0.75wt% polyphosphoric acid;

[0033] The geopolymer combined with silicon carbide refractory material prepared by the present invention has been tested to have an apparent porosity of 10-15%, a room temperature flexural strength of 40-50 MPa, a compressive strength of 250-300 MPa, and a residual flexural strength retention rate (thermal shock stability) of 80-90% (water-cooled at 1100°C for 3 times).

[0034] The above technical solutions only reflect the preferred technical solutions of the technical solutions of the present invention. Some changes that may be made to certain parts thereof by technicians in this technical field all reflect the principles of the present invention and fall within the protection scope of the present invention.

Claims

1. A geopolymer-bonded silicon carbide refractory material, characterized in that: The invention is composed of the following substances in weight percentage: 70-90 wt % of silicon carbide, 7-21 wt % of aluminum silicate powder, 1-3 wt % of phosphoric acid activator and 2-6 wt % of water as raw materials.

2. The method for preparing a geopolymer-bonded silicon carbide refractory material according to claim 1, characterized in that: The following steps are involved: Step 1: first mechanically mix aluminum silicate powder, phosphoric acid activator and water to obtain a geopolymer sol; Step 2: Stir the sol and silicon carbide evenly; press and form under 80-200 MPa, dry at 110°C for 48 hours, heat to 1200-1400°C at a rate of 2-10°C / min in air atmosphere, keep warm for 2-5 hours, and cool to room temperature with the furnace; Step 3: Prepare geopolymer-bonded silicon carbide refractory material.

3. The method for preparing a geopolymer-bonded silicon carbide refractory material according to claim 2, characterized in that: The SiC content in the silicon carbide is ≥98wt% and the particle size is ≤3mm.

4. The method for preparing a geopolymer-bonded silicon carbide refractory material according to claim 2, characterized in that: The aluminum silicate powder is a combination of one or more of pyrophyllite, kaolin, sillimanite, vermiculite and mica.

5. The method for preparing a geopolymer-bonded silicon carbide refractory material according to claim 2, characterized in that: The phosphoric acid activator is a combination of one or more of orthophosphoric acid, phosphorous acid, metaphosphoric acid and polyphosphoric acid.

Citation Information

Patent Citations

  • Silicon carbide ceramic product and preparation method

    CN102503431A

  • Preparation method of oxide combined SiC porous ceramic

    CN104072142A

  • Heat-conducting geopolymer composite material as well as preparation and application thereof

    CN111393056A

  • Method for preparing porous oxide microspheres by using geopolymer as binder

    CN112321297A

  • Phosphoric acid-based geopolymer semi-rigid base material and application thereof

    CN116750995A