Carbon-ceramic composite material as well as preparation method and application thereof
Through chemical vapor deposition and graphitization of carbon fiber preforms, combined with high-temperature impregnation and cracking steps, carbon-ceramic composite materials with moderate density are prepared, which solves the problems of complex process, high cost and insufficient braking performance in the existing technology, and achieves Efficient preparation and good braking performance of carbon-ceramic composites.
Patent Information
- Application Number
- CN202410762074.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
AI Technical Summary
The existing carbon-ceramic composite materials have complex preparation processes and high costs, and have weak braking energy absorption/heat dissipation capabilities and are prone to cracking, making it difficult to meet the braking needs of passenger cars.
Carbon fiber is woven into prefabricated parts, and through chemical vapor deposition, graphitization and impregnation pyrolysis steps, a carbon-ceramic composite material with moderate density is prepared, using polyacrylonitrile-based carbon fiber and pitch-based carbon fiber, with a volume ratio of 1 to 3:1. The fiber volume fraction is 25% to 35%. It is processed through acetone reflux, deionized water cleaning and vacuum drying, combined with chemical vapor deposition furnace and graphitization furnace, and finally vacuum impregnation and pyrolysis at high temperature.
The prepared carbon-ceramic composite material has a density of 1.9-2.0g/cm3, a moderate friction coefficient, good wear resistance, strong braking energy absorption/heat dissipation ability, not easy to crack, simple process, low cost, and good repeatability.
Smart Images

Figure CN118724604A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of fiber-reinforced ceramic composite materials, and in particular relates to a carbon-ceramic composite material and a preparation method and application thereof. Background Art
[0002] Braking materials are an important part of the brake actuation system of passenger cars and are crucial to driving safety and control experience. At present, the mainstream brake disc material for passenger cars is gray cast iron, but the thermal decay of gray cast iron is more serious. When the friction intensifies and leads to higher temperatures, the braking performance decreases and the braking distance is shortened. Compared with gray cast iron, carbon fiber reinforced carbon-silicon carbide composite materials (referred to as carbon ceramic composite materials) have the advantages of high strength, low density, stable friction performance, small friction, strong environmental adaptability, and long service life. It is a new generation of high-performance braking materials and has a wide range of applications and prospects in the fields of high-speed trains, aircraft, racing cars, and high-performance passenger car braking.
[0003] Chinese patent CN201910694425X discloses a method for preparing carbon ceramic friction material, which adopts a combination of PIP and RMI processes. In the RMI process, silicon powder and amorphous silicon carbide powder are used as silicon infiltration raw materials at the same time. Amorphous silicon carbide is obtained by pyrolysis of ceramic precursors at low temperature. The advantage of this method is that by adjusting the particle size and content of different silicon carbides in the material, the friction coefficient of the obtained carbon ceramic friction material is adjustable and stable, the wear amount is small, there is no obvious vibration during braking, and there is no large attenuation in the wet state in the later stage of friction. The disadvantages are complex process, high cost, uneven distribution of components, and easy to cause problems such as eccentric wear and cracking.
[0004] Chinese patent CN103511525A discloses a carbon ceramic brake pad for high-speed trains and a preparation method thereof, which controls the composition of carbon ceramic composite materials, uses low-density carbon fiber felt as a reinforcement, and prepares the carbon ceramic brake pad through subsequent high-temperature treatment, thermal gradient chemical vapor deposition carburizing treatment, catalytic graphitization treatment, and non-immersion melt infiltration process. This method has excellent mechanical and friction properties, stable braking, and strong environmental adaptability. The disadvantages are complex preparation process, high cost, long manufacturing cycle, insufficient heat dissipation performance, and easy cracking.
[0005] Therefore, it is necessary to provide a carbon-ceramic composite material with weak braking energy absorption / heat dissipation capability and not prone to cracking. Summary of the invention
[0006] In view of the above problems existing in the prior art, the first technical problem to be solved by the present invention is to provide a method for preparing a carbon-ceramic composite material, which has simple process, low cost, easy operation and good repeatability. The second technical problem to be solved by the present invention is to provide a carbon-ceramic composite material, which has a moderate friction coefficient, good wear resistance, strong braking energy absorption / heat dissipation capacity, and is not easy to crack. The third technical problem to be solved by the present invention is to provide an application of a carbon-ceramic composite material in passenger car braking, which is used for passenger car braking.
[0007] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a carbon-ceramic composite material comprises the following steps: firstly weaving carbon fibers into a 2.5-dimensional or 3-dimensional preform, placing the preform in a solvent for reflux, washing and drying the preform, then placing the preform in a chemical vapor deposition furnace to deposit pyrolytic carbon, performing graphitization treatment, and then impregnating and cracking the preform to finally obtain the carbon-ceramic composite material.
[0009] Furthermore, the carbon fiber is polyacrylonitrile-based carbon fiber and asphalt-based carbon fiber.
[0010] Furthermore, the volume ratio of the carbon fiber to the asphalt-based carbon fiber is 1 to 3:1.
[0011] Furthermore, the fiber volume fraction of the preform is 25% to 35%.
[0012] Furthermore, the reflux solvent is acetone.
[0013] Furthermore, the gas pressure in the chemical vapor deposition furnace is 2000-4000 Pa, the temperature in the furnace is 1000-1200°C, the volume ratio of the carbon source gas and the dilution gas in the furnace is 1:2-6, and the chemical vapor deposition time is 40-80 hours; the carbon source gas is a mixture of acetylene and natural gas in a volume ratio of 1:2-5, and the dilution gas is nitrogen.
[0014] Furthermore, the impregnation liquid is a mixed solution of polyaluminosilazane, polycarbosilane, toluene and silicon powder; the mass ratio of the polyaluminosilazane, polycarbosilane, toluene and silicon powder is 1-5:1-5:20-30:1.
[0015] Further, the specific steps are as follows:
[0016] 1) Mixing polyacrylonitrile-based carbon fiber and asphalt-based carbon fiber into a preform by weaving and braiding, the preform is in a 2.5-dimensional or 3-dimensional form, and the fiber volume fraction is 25% to 35%; wherein the volume ratio of the polyacrylonitrile-based carbon fiber to the asphalt-based carbon fiber is 1 to 3:1;
[0017] 2) placing the preform prepared in step 1) in a 70° C. acetone solution for reflux treatment for 5 to 8 hours, and after the reflux is completed, washing the preform with deionized water for 2 to 4 times, and then drying the washed preform in a 110° C. vacuum oven for 2 to 3 hours;
[0018] 3) The preform dried in step 2) is placed in a chemical vapor deposition furnace to deposit pyrolytic carbon to obtain a carbon having a density of 1.1 to 1.3 g / cm 3 C / C composite material; wherein the gas pressure in the chemical vapor deposition furnace is 2000-4000 Pa, the temperature in the furnace is 1000-1200° C., the volume ratio of the carbon source gas to the dilution gas in the furnace is 1:2-6, and the chemical vapor deposition time is 40-80 hours; the carbon source gas is a mixture of acetylene and natural gas in a volume ratio of 1:2-5, and the dilution gas is nitrogen;
[0019] 4) placing the C / C composite material prepared in step 3) in a graphitization furnace for heat treatment at a temperature of 2500 to 2800° C. for a time of 30 to 90 min, and the protective atmosphere in the furnace is argon;
[0020] 5) placing the graphitized C / C composite material in the impregnation solution for vacuum impregnation, and after the impregnation, performing high temperature cracking and heat preservation under a protective atmosphere, and repeating the impregnation cracking and heat preservation steps for 6 to 10 times to obtain a composite material with a density of 1.9 to 2.0 g / cm 3 A carbon-ceramic composite material; wherein the impregnation liquid is a mixed solution of polyaluminosilazane, polycarbosilane, toluene and silicon powder in a mass ratio of 1 to 5:1 to 5:20 to 30:1; the number average molecular weight of polyaluminosilazane and polycarbosilane is 1500 to 2000, and the particle size of the silicon powder is 30 to 50 nm; the impregnation vacuum degree is 100 to 500 Pa, the high-temperature cracking temperature is 900 to 1300°C, the protective atmosphere is argon, the heating rate during cracking is 3 to 8°C / min, and the insulation time is 2 to 3 hours.
[0021] The carbon-ceramic composite material is prepared by the method for preparing the carbon-ceramic composite material.
[0022] The application of the carbon-ceramic composite material in passenger car braking.
[0023] Beneficial effects: Compared with the prior art, the advantages of the present invention are:
[0024] (1) The carbon-ceramic composite material prepared by the present invention has a density of 1.9 to 2.0 g / cm 3 , moderate friction coefficient, good wear resistance, strong braking energy absorption / heat dissipation ability, and not easy to crack.
[0025] (2) The preparation method of the present invention is simple, easy to operate, has good repeatability and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a microscopic morphology of the carbon-ceramic composite material prepared by the present invention;
[0027] Figure 2 The XRD spectrum of the carbon-ceramic composite material prepared by the present invention is shown in FIG. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with specific embodiments.
[0029] Example 1
[0030] The preparation steps of carbon ceramic composite materials are as follows:
[0031] 1) Mixing polyacrylonitrile-based carbon fiber and asphalt-based carbon fiber in a volume ratio of 1:1 by weaving and braiding to form a preform; the preform is 2.5-dimensional and has a fiber volume fraction of 30%;
[0032] 2) placing the preform obtained in step 1) in an acetone solution at 70° C. for reflux treatment for 5 h. After the reflux is completed, the preform is washed three times with deionized water, and then the washed preform is placed in a vacuum oven at 110° C. for drying for 2 h.
[0033] 3) The preform dried in step 2) is placed in a chemical vapor deposition furnace to deposit pyrolytic carbon to obtain a density of 1.1 g / cm 3 C / C composite material; wherein the gas pressure in the chemical vapor deposition furnace is 2000Pa, the temperature in the furnace is 1050°C, the volume ratio of the carbon source gas and the dilution gas in the furnace is 1:3, and the chemical vapor deposition time is 50h; the carbon source gas is a mixture of acetylene and natural gas in a volume ratio of 1:2, and the dilution gas is nitrogen;
[0034] 4) placing the C / C composite material prepared in step 3) in a graphitization furnace for heat treatment at a temperature of 2500° C. for 60 min, and the protective atmosphere in the furnace is argon;
[0035] 5) The C / C composite material subjected to graphitization treatment in step 4) is placed in an impregnation solution for vacuum impregnation. After the impregnation is completed, it is subjected to high-temperature cracking and then heat preservation under a protective atmosphere. The impregnation cracking and heat preservation steps are repeated 8 times to obtain a density of 1.92 g / cm 3The carbon-ceramic composite material is prepared by: the impregnation liquid is a mixed solution of polyaluminosilazane, polycarbosilane, toluene and silicon powder in a mass ratio of 1:2:25:1; the number average molecular weights of polyaluminosilazane and polycarbosilane are 1800 and 1500 respectively, and the particle size of silicon powder is 45nm; the impregnation vacuum is 500Pa, the high temperature cracking temperature and the insulation temperature are both 1300℃, the protective atmosphere is argon, the heating rate during cracking is 5℃ / min, and the insulation time is 2h. The microscopic morphology of the prepared carbon-ceramic composite material is as follows: Figure 1 As shown in the XRD Figure 2 shown.
[0036] Figure 1 This is a microscopic morphology of the carbon-ceramic composite material prepared in the present invention. As can be seen from the figure, the middle circular area is the carbon fiber wrapped by SiAlNC, and the other areas are the ceramic matrix (including silicon carbide, silicon nitride and aluminum nitride).
[0037] Figure 2 This is the XRD spectrum of the carbon-ceramic composite material prepared by the present invention. As can be seen from the figure, the carbon-ceramic composite material contains β-Si3N4, AlN, α-SiC and β-SiC two kinds of silicon carbide with different structures.
[0038] Example 2
[0039] The preparation steps of carbon ceramic composite materials are as follows:
[0040] 1) Mixing polyacrylonitrile-based carbon fiber and asphalt-based carbon fiber in a volume ratio of 2:1 by weaving and braiding to form a preform; the preform is 3D and has a fiber volume fraction of 32%;
[0041] 2) placing the preform obtained in step 1) in an acetone solution at 70° C. for reflux treatment for 8 h. After the reflux is completed, the preform is washed twice with deionized water, and then the washed preform is placed in a vacuum oven at 110° C. for drying for 2 h.
[0042] 3) The preform dried in step 2) is placed in a chemical vapor deposition furnace to deposit pyrolytic carbon to obtain a density of 1.2 g / cm 3 C / C composite material; wherein the gas pressure in the chemical vapor deposition furnace is 2500Pa, the temperature in the furnace is 1100°C, the volume ratio of the carbon source gas and the dilution gas in the furnace is 1:4, and the chemical vapor deposition time is 70h; the carbon source gas is a mixture of acetylene and natural gas in a volume ratio of 1:1, and the dilution gas is nitrogen;
[0043] 4) placing the C / C composite material prepared in step 3) in a graphitization furnace for heat treatment at a temperature of 2700° C. for 35 min, and the protective atmosphere in the furnace is argon;
[0044] 5) The C / C composite material subjected to graphitization treatment in step 4) is placed in an impregnation solution for vacuum impregnation. After the impregnation is completed, it is subjected to high-temperature cracking and then heat preservation under a protective atmosphere. The impregnation cracking and heat preservation steps are repeated 10 times to obtain a density of 1.98 g / cm 3 A carbon-ceramic composite material; wherein the impregnation liquid is a mixed solution of polyaluminosilazane, polycarbosilane, toluene and silicon powder in a mass ratio of 2:3:30:1; the number average molecular weights of polyaluminosilazane and polycarbosilane are 1600 and 1800 respectively, and the particle size of the silicon powder is 30nm; the impregnation vacuum degree is 300Pa, the high-temperature cracking temperature and the insulation temperature are both 1250℃, the protective atmosphere is argon, the heating rate during cracking is 8℃ / min, and the insulation time is 3h.
Claims
1. A method for preparing a carbon-ceramic composite material, characterized in that: First, the carbon fiber is woven into a 2.5-dimensional or 3-dimensional preform, the preform is placed in a solvent for reflux, cleaned and dried, and then the preform is placed in a chemical vapor deposition furnace to deposit pyrolytic carbon, followed by graphitization treatment, and then impregnation and cracking to finally obtain a carbon-ceramic composite material.
2. The method for preparing the carbon-ceramic composite material according to claim 1, characterized in that: The carbon fibers are polyacrylonitrile-based carbon fibers and asphalt-based carbon fibers.
3. The method for preparing the carbon-ceramic composite material according to claim 2, characterized in that: The carbon fibers are polyacrylonitrile-based carbon fibers and asphalt-based carbon fibers in a volume ratio of 1 to 3:
1.
4. The method for preparing the carbon-ceramic composite material according to claim 1, characterized in that: The fiber volume fraction of the preform is 25% to 35%.
5. The method for preparing the carbon-ceramic composite material according to claim 1, characterized in that: The reflux solvent is acetone.
6. The method for preparing the carbon-ceramic composite material according to claim 1, characterized in that: The gas pressure in the chemical vapor deposition furnace is 2000-4000 Pa, the temperature in the furnace is 1000-1200° C., the volume ratio of the carbon source gas to the dilution gas in the furnace is 1:2-6, and the chemical vapor deposition time is 40-80 hours; the carbon source gas is a mixture of acetylene and natural gas in a volume ratio of 1:2-5, and the dilution gas is nitrogen.
7. The method for preparing the carbon-ceramic composite material according to claim 1, characterized in that: The impregnation liquid is a mixed solution of polyaluminosilazane, polycarbosilane, toluene and silicon powder; the mass ratio of the polyaluminosilazane, polycarbosilane, toluene and silicon powder is 1-5:1-5:20-30:
1.
8. The method for preparing the carbon-ceramic composite material according to claim 1, characterized in that: The specific steps are as follows: 1) Mixing polyacrylonitrile-based carbon fiber and asphalt-based carbon fiber into a preform by weaving and braiding, the preform is in a 2.5-dimensional or 3-dimensional form, and the fiber volume fraction is 25% to 35%; wherein the volume ratio of the polyacrylonitrile-based carbon fiber to the asphalt-based carbon fiber is 1 to 3:1; 2) placing the preform prepared in step 1) in a 70° C. acetone solution for reflux treatment for 5 to 8 hours, and after the reflux is completed, washing the preform with deionized water for 2 to 4 times, and then drying the washed preform in a 110° C. vacuum oven for 2 to 3 hours; 3) The preform dried in step 2) is placed in a chemical vapor deposition furnace to deposit pyrolytic carbon to obtain a carbon having a density of 1.1 to 1.3 g / cm 3 C / C composite material; wherein the gas pressure in the chemical vapor deposition furnace is 2000-4000 Pa, the temperature in the furnace is 1000-1200° C., the volume ratio of the carbon source gas to the dilution gas in the furnace is 1:2-6, and the chemical vapor deposition time is 40-80 hours; the carbon source gas is a mixture of acetylene and natural gas in a volume ratio of 1:2-5, and the dilution gas is nitrogen; 4) placing the C / C composite material prepared in step 3) in a graphitization furnace for heat treatment at a temperature of 2500 to 2800° C. for a time of 30 to 90 min, and the protective atmosphere in the furnace is argon; 5) placing the graphitized C / C composite material in the impregnation solution for vacuum impregnation, and after the impregnation, performing high temperature cracking and heat preservation under a protective atmosphere, and repeating the impregnation cracking and heat preservation steps for 6 to 10 times to obtain a composite material with a density of 1.9 to 2.0 g / cm 3 A carbon-ceramic composite material; wherein the impregnation liquid is a mixed solution of polyaluminosilazane, polycarbosilane, toluene and silicon powder in a mass ratio of 1 to 5:1 to 5:20 to 30:1; the number average molecular weight of polyaluminosilazane and polycarbosilane is 1500 to 2000, and the particle size of the silicon powder is 30 to 50 nm; the impregnation vacuum degree is 100 to 500 Pa, the high-temperature cracking temperature is 900 to 1300°C, the protective atmosphere is argon, the heating rate during cracking is 3 to 8°C / min, and the insulation time is 2 to 3 hours.
9. The carbon-ceramic composite material obtained by the method for preparing the carbon-ceramic composite material according to any one of claims 1 to 8.
10. Use of the carbon-ceramic composite material according to claim 9 in passenger car braking.
Citation Information
Patent Citations
Reparative coating and application thereof in repairing coating of silicon carbide-based composite material
CN105948819A
Carbon-ceramic composite material and preparation method for same through precursor impregnation
CN108129156A
Polyaluminosilazane, preparation method and application
CN115044047A
High-carbon SiCN precursor, impregnant, ceramic-based composite material and preparation method
CN117777468A
Polymetalosilazane, process of producing same, silicon nitride based ceramic, and process of preparing same
US5436398A