Method for preparing high-purity methyl acetate
By modifying the montmorillonite carrier catalyst, the purity and yield of methyl acetate are improved, the problems of short activity of traditional catalysts and environmental pollution are solved, and efficient and economical preparation of methyl acetate and reusable catalyst are achieved.
Patent Information
- Application Number
- CN202410715757.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
AI Technical Summary
The yield of high-purity methyl acetate prepared in the existing technology is low and the economic cost is high, and traditional catalysts such as concentrated sulfuric acid are harmful to the environment, have short catalyst activity, and are difficult to achieve efficient separation and recycling.
Modified montmorillonite is used as a carrier, and by filling with quaternary ammonium ions and silicon sources and loading p-toluenesulfonic acid, a catalyst with high catalytic activity is formed, which improves the reaction selectivity and separation efficiency, and realizes the recycling of the catalyst.
The purity and yield of methyl acetate are significantly improved, the reaction time is shortened, the risk of equipment corrosion is reduced, and the efficient and reusable catalyst is achieved, which is in line with the concept of green environmental protection.
Smart Images

Figure BDA0004875529510000051 
Figure BDA0004875529510000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparing methyl acetate, and particularly relates to a method for preparing high-purity methyl acetate. Background Art
[0002] Methyl acetate is an important solvent and organic chemical raw material. It is often used as a quick-drying solvent for cellulose nitrate and cellulose acetate in industry. It is widely used in paints, coatings, textiles, spices, medicine and food industries. It is also used in the manufacture of artificial leather and spices and as an extractant for oils and fats. High-purity methyl acetate can be used to synthesize acetic acid, acetic anhydride, methyl acrylate, vinyl acetate and acetamide. Methyl acetate is usually prepared with acetic acid and methanol as reaction raw materials and a catalyst. The addition of a catalyst can improve the reaction selectivity and reaction efficiency. Traditional processes generally use concentrated sulfuric acid as a catalyst. Concentrated sulfuric acid has the advantages of a wide range of sources and high catalytic activity. However, concentrated sulfuric acid is harmful to the environment and easily corrodes reaction equipment. In addition, its dehydration and strong oxidizing properties easily cause side reactions, which greatly increases the difficulty of separating methyl acetate.
[0003] At present, the catalysts commonly used in industry to replace concentrated sulfuric acid are mainly homogeneous systems of metals such as rhodium, nickel, and palladium. The catalytic activity of rhodium, nickel, palladium, and other metals is increased by loading them on a carrier. However, due to the common problems of homogeneous systems, it is difficult to separate the reaction product from the loaded catalyst, and the loss of rhodium active components is obvious. In the selection of carriers, generally high molecular organic matter or inorganic substances are used as carriers. The catalyst system using only high molecular organic matter as a carrier is not stable enough. The polymer is easy to degrade, resulting in the shedding of active metals, which leads to a significant decrease in catalyst activity. Compared with other inorganic substances (such as zeolite, molecular sieve, diatomaceous earth, TiO, silica gel, etc.), the catalyst prepared with activated carbon as a carrier has good catalytic activity, but the catalyst using only activated carbon as a carrier is easy to lose its catalytic activity. This is because activated carbon has low mechanical strength, poor thermal conductivity and thermal stability. Due to its short service life, the application of activated carbon carriers in industrial production is limited. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing high-purity methyl acetate, so as to solve the technical problems of low yield and high economic cost in the prior art for preparing high-purity methyl acetate.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing high-purity methyl acetate comprises the following steps:
[0007] 1) Preheating acetic acid, methanol and catalyst respectively through heat exchangers and then transporting them to a synthesis tower;
[0008] 2) The methyl acetate is extracted from the top of the synthesis tower, and after heat exchange in the distillation tower heat exchanger, it is transported to the distillation tower for separation, and then separated in the light removal tower and the heavy removal tower to obtain methyl acetate.
[0009] Furthermore, the molar ratio of acetic acid to methanol is 1.25-1.3:1.
[0010] Furthermore, the catalyst is prepared by the following steps:
[0011] Add the modified montmorillonite into deionized water, stir at room temperature for 1-1.5 hours, add p-toluenesulfonic acid, heat to 80-83° C., reflux and stir for 3-3.5 hours, cool and dry to obtain a catalyst.
[0012] Furthermore, the usage ratio of the modified montmorillonite, deionized water and p-toluenesulfonic acid is 1.9-2.2 g:10 mL:0.45-0.50 g.
[0013] Further, the modified montmorillonite is prepared by the following steps:
[0014] The montmorillonite is added into deionized water, heated to 50-52° C. and stirred until it is completely dispersed to obtain solution A; hexadecyltrimethylammonium bromide and anhydrous ethanol are added into deionized water, and after being evenly dispersed, ethyl orthosilicate is added and ultrasonically dissolved to obtain solution B; solution B is mixed with solution A, continuously stirred at 50-52° C., pH is adjusted, stirring is continued, suction filtering is performed, washing is performed until pH is neutral, drying is performed, calcining is performed, and cooling is performed to obtain modified montmorillonite.
[0015] Furthermore, the dosage ratio of montmorillonite to deionized water in solution A is 1.3-1.5 g: 20 mL.
[0016] Furthermore, the dosage ratio of hexadecyltrimethylammonium bromide, anhydrous ethanol, deionized water and ethyl orthosilicate in solution B is 1.6-1.8 g: 5 mL: 20 mL: 1.2-1.25 g.
[0017] Further, the pH is adjusted to 7.5-8.5.
[0018] Furthermore, the calcination temperature is 600-605°C, and the heating rate is 1°C / min.
[0019] Beneficial effects of the present invention:
[0020] The scheme of the present invention uses methanol and acetic acid as main raw materials, and improves the reaction selectivity under the catalytic system of the catalyst; the prepared catalyst has high mechanical strength and thermal stability, and its structure is not easily destroyed, so the recycling of the catalyst is realized; methyl acetate is synthesized in one step by reactive distillation, and the preparation method of the scheme of the present invention has the characteristics of good reaction selectivity, greatly improves the reaction efficiency and separation efficiency, and the product methyl acetate has high purity and high yield.
[0021] The self-made catalyst of the present invention first fills the montmorillonite interlayer structure with quaternary ammonium ions and silicon sources, and self-assembles between the layers to form a complete "liquid crystal-like" structure, which increases the interlayer spacing and specific surface area of the montmorillonite, thereby increasing the catalytic active sites; it also introduces abundant organic functional groups, so that the dispersibility of the montmorillonite is improved; and then p-toluenesulfonic acid is loaded on the modified montmorillonite to obtain a catalyst with high catalytic activity. Compared with the traditional catalyst concentrated sulfuric acid, the catalyst prepared in the present invention is used to catalyze the synthesis of methyl acetate, which greatly shortens the reaction time, improves the catalytic efficiency, and does not corrode the process equipment. In the preparation and synthesis of methyl acetate by the present invention, after the catalyst is reused 6 times, the catalytic activity is reduced, but methyl acetate with a mass fraction of 98.9%-99.1% can still be obtained. It can be seen that the catalyst still has a high catalytic activity, and at the same time has excellent reusability, economical cost, and conforms to the concept of green environmental protection. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] This embodiment provides a catalyst, and the preparation steps are as follows:
[0025] 1.9 g of modified montmorillonite was added into 10 mL of deionized water, stirred at room temperature for 1 h, 0.45 g of p-toluenesulfonic acid was added, the temperature was raised to 80° C., refluxed and stirred for 3 h, cooled, and dried at 110° C. for 12 h to obtain a catalyst.
[0026] The modified montmorillonite is prepared by the following steps:
[0027] 1.3 g of montmorillonite was added into 20 mL of deionized water, and the mixture was heated to 50°C and stirred until the mixture was completely dispersed to obtain solution A.
[0028] 1.6 g of hexadecyltrimethylammonium bromide and 5 mL of anhydrous ethanol were added to 20 mL of deionized water, and after being evenly dispersed, 1.22 g of ethyl orthosilicate was added and dissolved by ultrasonication to obtain solution B;
[0029] Solution B was mixed with solution A, and stirred continuously at 50°C for 6 hours. The pH was adjusted to 8.0, and stirring was continued. The mixture was filtered and washed until the pH was neutral. The mixture was dried at 110°C for 8 hours to obtain a modified montmorillonite precursor, which was then calcined in a muffle furnace, heated to 600°C at a heating rate of 1°C / min, maintained for 6 hours, and cooled to obtain a modified montmorillonite precursor.
[0030] Example 2
[0031] The only difference from Example 1 is that:
[0032] 2.0 g of modified montmorillonite was added into 10 mL of deionized water, stirred at room temperature for 1 h, 0.48 g of p-toluenesulfonic acid was added, the temperature was raised to 80° C., refluxed and stirred for 3.5 h, cooled, and dried at 110° C. for 12 h to obtain a catalyst.
[0033] The remaining materials and steps are the same as those in Example 1.
[0034] Example 3
[0035] The only difference from Example 1 is that:
[0036] 2.2 g of modified montmorillonite was added into 10 mL of deionized water, stirred at room temperature for 1 h, 0.50 g of p-toluenesulfonic acid was added, the temperature was raised to 82° C., refluxed and stirred for 3.3 h, cooled, and dried at 110° C. for 12 h to obtain a catalyst.
[0037] The remaining materials and steps are the same as those in Example 1.
[0038] Example 4
[0039] The present embodiment provides a method for preparing high-purity methyl acetate, comprising the following steps:
[0040] 1) acetic acid, methanol and the catalyst in Example 1 are respectively preheated through a heat exchanger and transported to a synthesis tower, wherein the molar ratio of acetic acid to methanol is 1.25:1;
[0041] 2) The methyl acetate is extracted from the top of the synthesis tower, and after heat exchange in the distillation tower heat exchanger, it is transported to the distillation tower for separation, and then separated in the light removal tower and the heavy removal tower to obtain methyl acetate.
[0042] Example 5
[0043] 1) acetic acid, methanol and the catalyst in Example 2 are respectively preheated through a heat exchanger and transported to a synthesis tower, wherein the molar ratio of acetic acid to methanol is 1.25:1;
[0044] 2) The methyl acetate is extracted from the top of the synthesis tower, and after heat exchange in the distillation tower heat exchanger, it is transported to the distillation tower for separation, and then separated in the light removal tower and the heavy removal tower to obtain methyl acetate.
[0045] Example 6
[0046] 1) acetic acid, methanol and the catalyst in Example 3 are respectively preheated through a heat exchanger and transported to a synthesis tower, wherein the molar ratio of acetic acid to methanol is 1.25:1;
[0047] 2) The methyl acetate is extracted from the top of the synthesis tower, and after heat exchange in the distillation tower heat exchanger, it is transported to the distillation tower for separation, and then separated in the light removal tower and the heavy removal tower to obtain methyl acetate.
[0048] Comparative Example 1
[0049] The only difference from Example 4 is that the catalyst in Example 4 is replaced by a commercially available concentrated sulfuric acid catalyst, and the remaining raw materials and steps are the same as those in Example 4.
[0050] The yield and purity of methyl acetate obtained in Examples 4 to 6 and Comparative Example 1 were tested, and the yield of methyl acetate after the catalyst was reused 6 times was detected. The test results are shown in Table 1:
[0051] Table 1
[0052]
[0053]
[0054] By observing and analyzing the results of Examples 4-6 and Comparative Example 1, it can be seen that the catalytic effect of methyl acetate synthesis using the homemade catalyst of the present invention is outstanding, the yield and purity of methyl acetate are excellent, and the catalyst obtained in the present invention has an excellent reuse rate and economic cost. In summary, it is shown that the preparation method of the present invention has good reaction selectivity, a high yield of methyl acetate, and economical cost.
[0055] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing high-purity methyl acetate, characterized in that: The following steps are involved: 1) Preheating acetic acid, methanol and catalyst respectively through heat exchangers and then transporting them to a synthesis tower; 2) The methyl acetate is extracted from the top of the synthesis tower, and after heat exchange in the distillation tower heat exchanger, it is transported to the distillation tower for separation, and then separated in the light removal tower and the heavy removal tower to obtain methyl acetate.
2. A method for preparing high-purity methyl acetate according to claim 1, characterized in that: The molar ratio of acetic acid to methanol is 1.25-1.3:
1.
3. A method for preparing high-purity methyl acetate according to claim 1, characterized in that: The catalyst is prepared by the following steps: Add the modified montmorillonite into deionized water, stir at room temperature for 1-1.5 hours, add p-toluenesulfonic acid, heat to 80-83° C., reflux and stir for 3-3.5 hours, cool and dry to obtain a catalyst.
4. A method for preparing high-purity methyl acetate according to claim 3, characterized in that: The usage ratio of modified montmorillonite, deionized water and p-toluenesulfonic acid is 1.9-2.2 g:10 mL:0.45-0.50 g.
5. A method for preparing high-purity methyl acetate according to claim 3, characterized in that: The modified montmorillonite is prepared by the following steps: The montmorillonite is added into deionized water, heated to 50-52° C. and stirred until it is completely dispersed to obtain solution A; hexadecyltrimethylammonium bromide and anhydrous ethanol are added into deionized water, and after being evenly dispersed, ethyl orthosilicate is added and ultrasonically dissolved to obtain solution B; solution B is mixed with solution A, continuously stirred at 50-52° C., pH is adjusted, stirring is continued, suction filtering is performed, washing is performed until pH is neutral, drying is performed, calcining is performed, and cooling is performed to obtain modified montmorillonite.
6. A method for preparing high-purity methyl acetate according to claim 5, characterized in that: The dosage ratio of montmorillonite to deionized water in solution A is 1.3-1.5 g:20 mL.
7. A method for preparing high-purity methyl acetate according to claim 5, characterized in that: The dosage ratio of hexadecyltrimethylammonium bromide, anhydrous ethanol, deionized water and ethyl orthosilicate in solution B is 1.6-1.8 g: 5 mL: 20 mL: 1.2-1.25 g.
8. A method for preparing high-purity methyl acetate according to claim 5, characterized in that: The pH was adjusted to 7.5-8.
5.