Epoxy curing agent and preparation method thereof

The water-based epoxy curing agent prepared by using raw materials such as vegetable oil polyol and isocyanate solves the problem of poor impact resistance of traditional epoxy curing agents, achieves a combination of increased flexibility and environmental protection properties, and is suitable for concrete coatings and other fields.

CN118725233APending Publication Date: 2024-10-01SHAOGUAN DEKEMEI CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410928487.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional epoxy curing agents have poor impact resistance and are difficult to meet the strict requirements of engineering technology. Especially in concrete coatings, flexibility needs to be improved to ensure crack following.

Method used

Using raw materials such as vegetable oil polyols, isocyanates and polythiol compounds, a water-based epoxy curing agent with excellent flexibility is prepared through addition reaction and neutralization reaction to form a polyurethane resin, which combines isocyanate and thiol chemistry to give the film-forming material excellent Flexibility.

Benefits of technology

The flexibility of the epoxy curing agent is improved, and an environmentally friendly water-based resin is formed, which avoids pollution by volatile organic compounds. The raw materials are renewable and low-priced, meeting environmental protection requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an epoxy curing agent and a preparation method thereof. The epoxy curing agent is prepared from the following raw materials in parts by weight: 300 to 670 parts of vegetable oil polyol, 10 to 45 parts of micromolecular polyol, 160 to 250 parts of diisocyanate, 20 to 48 parts of hydrophilic chain extender, 0.8 to 2.0 parts of catalyst, 35 to 95 parts of multi-sulfhydryl compound and 10 to 35 parts of amine. When the epoxy curing agent is applied to a coating, a paint film can have relatively good flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and particularly relates to an epoxy curing agent and a preparation method thereof. Background Art

[0002] Two-component epoxy systems have excellent adhesion, mechanical strength, electrical insulation and other properties, and are therefore widely used in various industrial fields of the national economy. However, traditional epoxy curing agents are mostly small-molecule polyamine structures, or contain a large number of aromatic ring structures, with high glass transition temperatures, brittleness, and poor impact resistance, which limits their application and makes it difficult to meet the increasingly stringent requirements of many engineering technologies. For example, epoxy curing agents used in concrete coatings need to have good ductility to ensure their crack tracking and achieve effective protection of concrete. Therefore, how to improve the flexibility of epoxy curing agents has become an important research direction in epoxy resin technology.

[0003] With the increasing perfection of environmental regulations and the increasing environmental protection requirements in the world, traditional solvent-based coatings have been greatly impacted by the emission of volatile organic compounds, and their market share is shrinking rapidly, while water-based coatings, UV-curable coatings, high-solid coatings and powder coatings with environmental protection characteristics are growing rapidly. Among them, water-based coatings are developing rapidly because of their environmental protection, coating performance close to traditional coatings, and small changes to existing coating technology. In the past few years, water-based coatings have developed very rapidly in wood, leather, automobile, industry and other industries. At present, there is no epoxy curing agent with good flexibility on the market, and it is of great significance to develop an epoxy curing agent with good flexibility. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides an epoxy curing agent and a preparation method thereof, which can make the paint film have good flexibility when used in the paint.

[0005] The above technical objectives of the present invention are achieved through the following technical solutions:

[0006] An epoxy curing agent comprises the following raw materials in parts by weight: 300-670 parts of vegetable oil polyol, 10-45 parts of small molecule polyol, 160-250 parts of diisocyanate, 20-48 parts of hydrophilic chain extender, 0.8-2.0 parts of catalyst, 35-95 parts of polythiol compound and 10-35 parts of amine.

[0007] Preferably, the vegetable oil polyol is at least one of castor oil polyol, soybean oil polyol and palm oil polyol.

[0008] Preferably, the small molecule polyol is at least one of ethylene glycol, propylene glycol, diethylene glycol, 1,4-butanediol and trimethylolpropane.

[0009] Preferably, the diisocyanate is at least one of toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and tetramethylxylylene diisocyanate.

[0010] Preferably, the hydrophilic chain extender is dimethylolpropionic acid.

[0011] Preferably, the catalyst is at least one of isopropyl titanate, stannous octoate and dibutyltin dilaurate.

[0012] Preferably, the polythiol compound is at least one of diol di(3-mercaptopropionate), trimethylolpropane tri(3-mercaptopropionate) and pentaerythritol tetra(3-mercaptopropionate).

[0013] Preferably, the amine is at least one of triethanolamine and N,N-dimethylethanolamine.

[0014] Preferably, the epoxy curing agent has a solid content of 40%-50%, a viscosity of 1000-10000 mPa·S, and an acid value of 10-30 mgKOH / g.

[0015] A method for preparing the epoxy curing agent as described above comprises the following steps:

[0016] (1) dissolving a vegetable oil polyol, a small molecule polyol, a diisocyanate and a hydrophilic chain extender in an organic solvent, adding a catalyst to cause an addition reaction, and obtaining an isocyanate-terminated polyurethane prepolymer;

[0017] (2) mixing the isocyanate-terminated polyurethane prepolymer obtained in step (1) with a polythiol compound to obtain a thiol-terminated structural resin containing an urethane structure;

[0018] (3) adding amine to the thiol-terminated resin obtained in step (2) for neutralization reaction, adding water dropwise for phase inversion, and removing the organic solvent to obtain a thiol-terminated water-based resin, which is the epoxy curing agent.

[0019] Preferably, the organic solvent is at least one of acetone and butanone.

[0020] Preferably, in step (1), the dissolving temperature is 40-100°C.

[0021] Preferably, in step (1), the temperature of the addition reaction is 50-100° C., and the time of the addition reaction is 2-5 h.

[0022] Preferably, in step (2), the reaction temperature is 50-80°C, and the reaction time is 3-5h.

[0023] Preferably, in step (3), the temperature of the neutralization reaction is 50-80°C.

[0024] Preferably, in step (3), the temperature during the phase inversion is maintained at the same temperature as during the neutralization reaction, and the phase inversion time is 0.5-3h.

[0025] Preferably, in step (3), the method for removing the organic solvent is by distilling under reduced pressure after heating.

[0026] The beneficial effects of the present invention are:

[0027] The epoxy curing agent of the present invention is a water-based resin, which will not cause volatile organic pollution during use and is environmentally friendly. It is chemically combined with isocyanate and thiol to give the final film-forming material polyurethane excellent flexibility. In addition, it uses vegetable oil polyol as a raw material, which has the advantages of low price, environmental protection, and renewable raw materials compared to traditional petrochemical diol products as raw materials. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific embodiments.

[0029] Embodiment 1:

[0030] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: soybean oil polyol: 398g, 1,4-butanediol: 40.5g, isophorone diisocyanate: 222g, dihydroxymethylpropionic acid: 37.4g, dibutyltin dilaurate: 1.4g, trimethylolpropane tris(3-mercaptopropionate): 63.5g, and N,N-dimethylethanolamine: 21g.

[0031] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0032] (1) 100 g of acetone, 398 g of soybean oil polyol, 40.5 g of 1,4-butanediol, 37.4 g of dimethylol propionic acid, and 222 g of isophorone diisocyanate were put into a reactor, the temperature was raised to 60° C. to dissolve the materials, 1.4 g of dibutyltin dilaurate was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0033] (2) adding 63.5 g of trimethylolpropane tris(3-mercaptopropionate) into the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0034] (3) maintaining the reaction temperature at 60°C, adding 21g of N,N-dimethylethanolamine to the reactor for neutralization, after neutralization, adding 990g of deionized water to the reactor for phase inversion for 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 44.1%, a viscosity of 1500mPa·S, and an acid value of 20.0mgKOH / g.

[0035] Embodiment 2:

[0036] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: 334 g of castor oil polyol, 24.1 g of trimethylolpropane, 174 g of toluene diisocyanate, 26.5 g of dimethylolpropionic acid, 1.1 g of dibutyltin dilaurate, 36.0 g of trimethylolpropane tris(3-mercaptopropionate), and 15 g of N,N-dimethylethanolamine.

[0037] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0038] (1) 85 g of acetone, 334 g of castor oil polyol, 24.1 g of trimethylolpropane, 26.5 g of dimethylolpropionic acid, and 174 g of toluene diisocyanate were placed in a reaction kettle, the temperature was raised to 60° C. to dissolve the materials, 1.1 g of dibutyltin dilaurate catalyst was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0039] (2) adding 36.0 g of trimethylolpropane tris(3-mercaptopropionate) into the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0040] (3) maintaining the reaction temperature at 60°C, adding 15g of N,N-dimethylethanolamine to the reactor for neutralization, and after neutralization, adding 820g of deionized water to the reactor for phase inversion over 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 42.7%, a viscosity of 5300mPa·S, and an acid value of 18.1mgKOH / g.

[0041] Embodiment 3:

[0042] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: 353 g of palm oil polyol, 13.6 g of ethylene glycol, 168 g of hexamethylene diisocyanate, 27.9 g of dihydroxymethylpropionic acid, 1.1 g of dibutyltin dilaurate, 46.8 g of trimethylolpropane tris(3-mercaptopropionate), and 16 g of N,N-dimethylethanolamine.

[0043] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0044] (1) 90 g of acetone, 353 g of palm oil polyol, 13.6 g of ethylene glycol, 27.9 g of dimethylol propionic acid, and 168 g of hexamethylene diisocyanate were placed in a reaction kettle, the temperature was raised to 60° C. to dissolve the materials, 1.1 g of dibutyltin dilaurate catalyst was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0045] (2) adding 46.8 g of trimethylolpropane tris(3-mercaptopropionate) to the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0046] (3) maintaining the reaction temperature at 60°C, adding 16g of N,N-dimethylethanolamine to the reactor for neutralization, and after neutralization, adding 820g of deionized water to the reactor for phase inversion for 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 43.3%, a viscosity of 1100mPa·S, and an acid value of 18.6mgKOH / g.

[0047] Embodiment 4:

[0048] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: soybean oil polyol: 561g, diethylene glycol: 36.0g, isophorone diisocyanate: 222g, dimethylolpropionic acid: 42.6g, isopropyl titanate: 1.7g, trimethylolpropane tris(3-mercaptopropionate): 56.5g, and N,N-dimethylethanolamine: 24g.

[0049] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0050] (1) 110 g of acetone, 561 g of soybean oil polyol, 36.0 g of diethylene glycol, 42.6 g of dimethylol propionic acid, and 222 g of isophorone diisocyanate were placed in a reactor, the temperature was raised to 60° C. to dissolve the materials, 1.7 g of isopropyl titanate catalyst was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0051] (2) adding 56.5 g of trimethylolpropane tris(3-mercaptopropionate) to the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0052] (3) maintaining the reaction temperature at 60°C, adding 24g of N,N-dimethylethanolamine to the reactor for neutralization, and after neutralization, adding 1200g of deionized water to the reactor for phase inversion for 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 44.0%, a viscosity of 2200mPa·S, and an acid value of 18.9mgKOH / g.

[0053] Embodiment 5:

[0054] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: soybean oil polyol: 461g, 1,4-butanediol: 28.8g, tetramethylxylene diisocyanate: 244g, dihydroxymethylpropionic acid: 42.6g, stannous octoate: 1.7g, trimethylolpropane tris(3-mercaptopropionate): 73.7g, and N,N-dimethylethanolamine: 24g.

[0055] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0056] (1) 110 g of acetone, 461 g of soybean oil polyol, 28.8 g of 1,4-butanediol, 42.6 g of dimethylol propionic acid, and 244 g of tetramethylxylylene diisocyanate were placed in a reaction kettle, the temperature was raised to 60° C. to dissolve the materials, 1.7 g of stannous octoate catalyst was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0057] (2) adding 73.7 g of trimethylolpropane tris(3-mercaptopropionate) to the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0058] (3) maintaining the reaction temperature at 60°C, adding 24g of N,N-dimethylethanolamine to the reactor for neutralization, and after neutralization, adding 1240g of deionized water to the reactor for phase inversion for 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 41.4%, a viscosity of 3500mPa·S, and an acid value of 20.3mgKOH / g.

[0059] Embodiment 6:

[0060] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: soybean oil polyol: 461g, 1,4-butanediol: 28.8g, tetramethylxylene diisocyanate: 244g, dihydroxymethylpropionic acid: 42.6g, dibutyltin dilaurate: 1.7g, pentaerythritol tetrakis (3-mercaptopropionate): 90.4g, and N,N-dimethylethanolamine: 24g.

[0061] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0062] (1) 110 g of acetone, 461 g of soybean oil polyol, 28.8 g of 1,4-butanediol, 42.6 g of dimethylol propionic acid, and 244 g of tetramethylxylene diisocyanate were put into a reaction kettle, the temperature was raised to 60° C. to dissolve the materials, 1.7 g of dibutyltin dilaurate catalyst was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0063] (2) adding 90.4 g of pentaerythritol tetrakis(3-mercaptopropionate) to the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0064] (3) maintaining the reaction temperature at 60°C, adding 24g of N,N-dimethylethanolamine to the reactor for neutralization, after neutralization, adding 1240g of deionized water to the reactor for phase inversion for 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 41.9%, a viscosity of 4200mPa·S, and an acid value of 19.9mgKOH / g.

[0065] Embodiment 7:

[0066] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: soybean oil polyol: 312g, castor oil polyol: 93g, 1,4-butanediol: 34.2g, tetramethylxylene diisocyanate: 244g, dihydroxymethylpropionic acid: 37.4g, dibutyltin dilaurate: 1.4g, pentaerythritol tetrakis (3-mercaptopropionate): 54.1g, and N,N-dimethylethanolamine: 21g.

[0067] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0068] (1) 100 g of acetone, 312 g of soybean oil polyol, 93 g of castor oil polyol, 34.2 g of 1,4-butanediol, 37.4 g of dimethylol propionic acid, and 244 g of tetramethylxylene diisocyanate were put into a reaction kettle, the temperature was raised to 60° C. to dissolve the materials, 1.4 g of dibutyltin dilaurate catalyst was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0069] (2) adding 54.1 g of pentaerythritol tetrakis(3-mercaptopropionate) to the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0070] (3) maintaining the reaction temperature at 60°C, adding 21g of N,N-dimethylethanolamine to the reactor for neutralization, and after neutralization, adding 1020g of deionized water to the reactor for phase inversion for 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 43.9%, a viscosity of 3200mPa·S, and an acid value of 19.6mgKOH / g.

[0071] Embodiment 8:

[0072] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: soybean oil polyol: 249g, castor oil polyol: 139g, 1,4-butanediol: 34.2g, isophorone diisocyanate: 222g, dihydroxymethylpropionic acid: 31.9g, dibutyltin dilaurate: 1.3g, pentaerythritol tetrakis (3-mercaptopropionate): 77.8g, and N,N-dimethylethanolamine: 18g.

[0073] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0074] (1) 90 g of acetone, 249 g of soybean oil polyol, 139 g of castor oil polyol, 34.2 g of 1,4-butanediol, 31.9 g of dimethylol propionic acid, and 222 g of isophorone diisocyanate were added to a reactor, the temperature was raised to 60° C. to dissolve the materials, 1.3 g of dibutyltin dilaurate catalyst was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0075] (2) adding 77.8 g of pentaerythritol tetrakis(3-mercaptopropionate) into the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0076] (3) maintaining the reaction temperature at 60°C, adding 18g of N,N-dimethylethanolamine to the reactor for neutralization, after neutralization, adding 950g of deionized water to the reactor for phase inversion for 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 44.9%, a viscosity of 3600mPa·S, and an acid value of 17.2mgKOH / g.

[0077] Embodiment 9:

[0078] An epoxy curing agent, characterized in that it comprises the following raw materials in parts by weight: soybean oil polyol: 208g, palm oil polyol: 185g, 1,4-butanediol: 28.8g, isophorone diisocyanate: 222g, dihydroxymethylpropionic acid: 31.9g, dibutyltin dilaurate: 1.3g, pentaerythritol tetrakis (3-mercaptopropionate): 69.9g, and triethanolamine: 31g.

[0079] The preparation method of the epoxy curing agent as described above comprises the following steps:

[0080] (1) 90 g of acetone, 208 g of soybean oil polyol, 185 g of palm oil polyol, 28.8 g of 1,4-butanediol, 31.9 g of dimethylol propionic acid, and 222 g of isophorone diisocyanate were added to a reactor, the temperature was raised to 60° C. to dissolve the materials, 1.3 g of dibutyltin dilaurate catalyst was added, the temperature was raised to 70° C. to react for 3 hours, and an isocyanate-terminated polyurethane prepolymer was obtained.

[0081] (2) adding 69.9 g of pentaerythritol tetrakis(3-mercaptopropionate) to the obtained isocyanate-terminated polyurethane prepolymer into a reaction kettle, and reacting at 60° C. for 4 hours to obtain a brown-yellow mercapto-terminated polyurethane resin;

[0082] (3) maintaining the reaction temperature at 60°C, adding 31g of triethanolamine to the reactor for neutralization, after neutralization, adding 950g of deionized water to the reactor for phase inversion over 2 hours, keeping the temperature for 1 hour, raising the temperature to 80°C, and removing acetone by vacuum distillation to obtain a light yellow, blue-light-capped thiol-terminated water-based resin. The raw materials described in this embodiment are all commercially available raw materials, and the prepared product has a solid content of 45.0%, a viscosity of 4200mPa·S, and an acid value of 17.1mgKOH / g.

[0083] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. An epoxy curing agent, characterized in that: The invention comprises the following raw materials in parts by weight: 300-670 parts of vegetable oil polyol, 10-45 parts of small molecule polyol, 160-250 parts of diisocyanate, 20-48 parts of hydrophilic chain extender, 0.8-2.0 parts of catalyst, 35-95 parts of polythiol compound and 10-35 parts of amine.

2. An epoxy curing agent according to claim 1, characterized in that: The vegetable oil polyol is at least one of castor oil polyol, soybean oil polyol and palm oil polyol.

3. An epoxy curing agent according to claim 1, characterized in that: The small molecule polyol is at least one of ethylene glycol, propylene glycol, diethylene glycol, 1,4-butanediol and trimethylolpropane.

4. An epoxy curing agent according to claim 1, characterized in that: The diisocyanate is at least one of toluene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate and tetramethylxylylene diisocyanate.

5. An epoxy curing agent according to claim 1, characterized in that: The hydrophilic chain extender is dimethylol propionic acid.

6. An epoxy curing agent according to claim 1, characterized in that: The catalyst is at least one of isopropyl titanate, stannous octoate and dibutyltin dilaurate.

7. An epoxy curing agent according to claim 1, characterized in that: The polythiol compound is at least one of diol di(3-mercaptopropionate), trimethylolpropane tri(3-mercaptopropionate) and pentaerythritol tetra(3-mercaptopropionate).

8. An epoxy curing agent according to claim 1, characterized in that: The amine is at least one of triethanolamine and N,N-dimethylethanolamine.

9. An epoxy curing agent according to claim 1, characterized in that: The epoxy curing agent has a solid content of 40%-50%, a viscosity of 1000-10000 mPa·S, and an acid value of 10-30 mgKOH / g.

10. A method for preparing the epoxy curing agent according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) dissolving a vegetable oil polyol, a small molecule polyol, a diisocyanate and a hydrophilic chain extender in an organic solvent, adding a catalyst to cause an addition reaction, and obtaining an isocyanate-terminated polyurethane prepolymer; (2) mixing the isocyanate-terminated polyurethane prepolymer obtained in step (1) with a polythiol compound to obtain a thiol-terminated structural resin containing an urethane structure; (3) adding amine to the thiol-terminated resin obtained in step (2) for neutralization reaction, adding water dropwise for phase inversion, and removing the organic solvent to obtain a thiol-terminated water-based resin, which is the epoxy curing agent.